0% found this document useful (0 votes)
14 views84 pages

PC (7TH SEM)

The document is a lecture note on Prestressed Concrete, covering its principles, advantages, materials, methods, and design considerations. It includes detailed modules on prestressing systems, beam design, and the selection of prestressed concrete members, as well as the stresses involved in prestressed members. The document also discusses the historical background and various applications of prestressed concrete in construction.

Uploaded by

maddoxkumar001
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
0% found this document useful (0 votes)
14 views84 pages

PC (7TH SEM)

The document is a lecture note on Prestressed Concrete, covering its principles, advantages, materials, methods, and design considerations. It includes detailed modules on prestressing systems, beam design, and the selection of prestressed concrete members, as well as the stresses involved in prestressed members. The document also discusses the historical background and various applications of prestressed concrete in construction.

Uploaded by

maddoxkumar001
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
You are on page 1/ 84

Prestressed Concrete

B.Tech,
SPINTRONIC TECHNOLOGY AND ADVANCE RESEARCH

Lecture Note
on
Prestressed Concrete
Prepared By:
Asst.Prof Prabhudatta Senapati

1 P.Senapati
Prestressed Concrete
B.Tech,

Module I:
Prestressing system, materials and codes: Basic concept, Losses of
prestress, analysis of prestress and bending stresses. Need for high
strength steel and concrete. Advantages and applications. Pre-
tensioning and post tensioning systems.
Module II: Design of beams : Analysis and design of section for bending
and shear, pressure line, concept of load balancing, cracking
moment, bending of cables, limit state analysis and design,
anchorage zone stresses, design of end block, Application to bridges.
Module III: Selection of prestress concrete members, short term and
long term deflections of uncracked members.
Module IV: Flexural strength of prestressed concrete
sections,Continuous beams, Design concept concordancy of cables,
Secondary design consideration
Module V: Design pre-tensioned and post tensioned beam.

Books: [1] Prestressed Concrete, N Krishna Raju, Tata McGraw-Hill


[2] Design of Prestressed Concrete Structures, T Y Lin, Ned H Burns, John
Wiley & Sons
[3] Prestressed Concrete Structures, P. Dayaratnam, P. Sarah,Medtech
Publisher

2 P.Senapati
Prestressed Concrete
B.Tech,

1. Introduction

1.1 Background
The idea of prestressed concrete has been around since the latter decades of the 19th
century, but its use was limited by the quality of the materials at the time. It took until
the 1920s and ‘30s for its materials development to progress to a level where
prestressed concrete could be used with confidence. Freyssinet in France, Magnel in
Belgium and Hoyer in Germany were the principle developers.

The idea of prestressing has also been applied to many other forms, such as:
• Wagon wheels;
• Riveting;
• Barrels, i.e. the coopers trade;
In these cases heated metal is made to just fit an object. When the metal cools it
contracts inducing prestress into the object.

3 P.Senapati
Prestressed Concrete
B.Tech,

1.2 Basic Principle of Prestressing

Basic Example

The classic everyday example of prestressing is this: a row of books can be lifted by
squeezing the ends together:

The structural explanation is that the row of books has zero tensile capacity. Therefore
the ‘beam’ of books cannot even carry its self weight. To overcome this we provide an
external initial stress (the prestress) which compresses the books together. Now they
can only separate if the tensile stress induced by the self weight of the books is greater
than the compressive prestress introduced.

Concrete

Concrete is very strong in compression but weak in tension. In an ordinary concrete


beam the tensile stress at the bottom:

4 P.Senapati
Prestressed Concrete
B.Tech,

are taken by standard steel reinforcement:

But we still get cracking, which is due to both bending and shear:

In prestressed concrete, because the prestressing keeps the concrete in compression,


no cracking occurs. This is often preferable where durability is a concern.

5 P.Senapati
Prestressed Concrete
B.Tech,

1.3 Advantages of Prestressed Concrete


The main advantages of prestressed concrete (PSC) are:

Smaller Section Sizes


Since PSC uses the whole concrete section, the second moment of area is bigger and
so the section is stiffer:

N A
N A

RC PSC

Smaller Deflections
The larger second moment of area greatly reduces deflections for a given section size.

Increased Spans
The smaller section size reduces self weight. Hence a given section can span further
with prestressed concrete than it can with ordinary reinforced concrete.

Durability
Since the entire section remains in compression, no cracking of the concrete can
occur and hence there is little penetration of the cover. This greatly improves the long-
term durability of structures, especially bridges and also means that concrete tanks can
be made as watertight as steel tanks, with far greater durability.

6 P.Senapati
Prestressed Concrete
B.Tech,

1.4 Materials

Concrete

The main factors for concrete used in PSC are:


• Ordinary portland cement-based concrete is used but strength usually greater
than 50 N/mm2;
• A high early strength is required to enable quicker application of prestress;
• A larger elastic modulus is needed to reduce the shortening of the member;
• A mix that reduces creep of the concrete to minimize losses of prestress;

You can see the importance creep has in PSC from this graph:

7 P.Senapati
Prestressed Concrete
B.Tech,

Steel

The steel used for prestressing has a nominal yield strength of between 1550 to 1800
N/mm2. The different forms the steel may take are:
• Wires: individually drawn wires of 7 mm diameter;
• Strands: a collection of wires (usually 7) wound together and thus having a
diameter that is different to its area;
• Tendon: A collection of strands encased in a duct – only used in post-
tensioning;
• Bar: a specially formed bar of high strength steel of greater than 20 mm
diameter.

Prestressed concrete bridge beams typically use 15.7 mm diameter (but with an area
of 150 mm2)7-wire super strand which has a breaking load of 265 kN.

8 P.Senapati
Prestressed Concrete
B.Tech,

9 P.Senapati
Prestressed Concrete
B.Tech,

1.5 Methods of Prestressing


There are two methods of prestressing:
• Pre-tensioning: Apply prestress to steel strands before casting concrete;
• Post-tensioning: Apply prestress to steel tendons after casting concrete.

Pre-tensioning

This is the most common form for precast sections. In Stage 1 the wires or strands are
stressed; in Stage 2 the concrete is cast around the stressed wires/strands; and in
Stage 3 the prestressed in transferred from the external anchorages to the concrete,
once it has sufficient strength:

10 P.Senapati
Prestressed Concrete
B.Tech,

In pre-tensioned members, the strand is directly bonded to the concrete cast around it.
Therefore, at the ends of the member, there is a transmission length where the strand
force is transferred to the concrete through the bond:

At the ends of pre-tensioned members it is sometimes necessary to debond the strand


from the concrete. This is to keep the stresses within allowable limits where there is
little stress induced by self with or other loads:

11 P.Senapati
Prestressed Concrete
B.Tech,

Post-tensioned

In this method, the concrete has already set but has ducts cast into it. The strands or
tendons are fed through the ducts (Stage 1) then tensioned (Stage 2) and then anchored
to the concrete (Stage 3):

The anchorages to post-tensioned members must distribute a large load to the concrete,
and must resist bursting forces as a result. A lot of ordinary reinforcement is often
necessary.

A typical tendon anchorage is:

12 P.Senapati
Prestressed Concrete
B.Tech,

And the end of a post-tensioned member has reinforcement such as:

13 P.Senapati
Prestressed Concrete
B.Tech,

Losses

From the time the prestress is applied, the prestress force gradually reduces over time
to an equilibrium level. The sources of these losses depend on the method by which
prestressing is applied.

In both methods:
• The member shortens due to the force and this relieves some of the prestress;
• The concrete shrinks as it further cures;
• The steel ‘relaxes’, that is, the steel stress reduces over time;
• The concrete creeps, that is, continues to strain over time.

In post-tensioning, there are also losses due to the anchorage (which can ‘draw in’ an
amount) and to the friction between the tendons and the duct and also initial
imperfections in the duct setting out.

For now, losses will just be considered as a percentage of the initial prestress.

14 P.Senapati
Prestressed Concrete
B.Tech,

1.6 Uses of Prestressed Concrete


There are a huge number of uses:
• Railway Sleepers;
• Communications poles;
• Pre-tensioned precast “hollowcore” slabs;
• Pre-tensioned Precast Double T units - for very long spans (e.g., 16 m span for
car parks);
• Pre-tensioned precast inverted T beam for short-span bridges;
• Pre-tensioned precast PSC piles;
• Pre-tensioned precast portal frame units;
• Post-tensioned ribbed slab;
• In-situ balanced cantilever construction - post-tensioned PSC;
• This is “glued segmental” construction;
• Precast segments are joined by post-tensioning;
• PSC tank - precast segments post-tensioned together on site. Tendons around
circumference of tank;
• Barges;
• And many more.

15 P.Senapati
Prestressed Concrete
B.Tech,

2. Stresses in Prestressed Members

2.1 Background
The codes of practice limit the allowable stresses in prestressed concrete. Most of the
work of PSC design involves ensuring that the stresses in the concrete are within the
permissible limits.

Since we deal with allowable stresses, only service loading is used, i.e. the SLS case.
For the SLS case, at any section in a member, there are two checks required:

At Transfer
This is when the concrete first feels the prestress. The concrete is less strong but the
situation is temporary and the stresses are only due to prestress and self weight.

At Service
The stresses induced by the SLS loading, in addition to the prestress and self weight,
must be checked. At service stage, the concrete has its full strength but losses will have
occurred and so the prestress force is reduced.

The ultimate capacity at ULS of the PSC section (as for RC) must also be checked. If
there is insufficient capacity, you can add non-prestressed reinforcement. This often
does not govern.

16 P.Senapati
Prestressed Concrete
B.Tech,

Notation

For a typical prestressed section:

We have:

Zt Section modulus, top fibre = I yt ;


Zb Section modulus, bottom fibre = −I yb (taken to be negative);

ftt Allowable tensile stress at transfer;


ftc Allowable compressive stress at transfer;
fst Allowable tensile stress in service;
fsc Allowable compressive stress ain service;
Mt The applied moment at transfer;
Ms The applied moment in service;

 The ratio of prestress after losses (service) to prestress before losses, (transfer).

17 P.Senapati
Prestressed Concrete
B.Tech,

Allowable Stresses
Concrete does have a small tensile strength and this can be recognized by the designer.
In BS 8110, there are 3 classes of prestressed concrete which depend on the level of
tensile stresses and/or cracking allowed:

Stresses Class 1 Class 2 Class 3

0.45 fci for pre-tensioned members


Tension: ftt 2
1 N/mm
At transfer

0.36 fci for post-tensioned members

Compression: ftc 0.5 fci *

0.45 fci (pre)


Tension: fst 2
0 N/mm See code table
In service

0.36 fci (post)

Compression: fsc 0.33 fcu

* there are other requirements for unusual cases – see code

18 P.Senapati
Prestressed Concrete
B.Tech,

2.2 Basic Principle of Prestressed Concrete

Theoretical Example

Consider the basic case of a simply-supported beam subjected to a UDL of w kN/m:

A B
C
L
VA VB

In this case, we have the mid-span moment as:


b

wL2
MC =
8
d

Also, if we assume a rectangular section as shown, we have


the following section properties:

bd 3
A = bd I=
12 2
bd 2 bd
Zt = Zb =
6 6

Therefore the stresses at C are:

MC MC
t = =
Z  b
Z
t b

19 P.Senapati
Prestressed Concrete
B.Tech,

Case I
If we take the beam to be constructed of plain concrete (no reinforcement) and we
neglect the (small) tensile strength of concrete ( ft = 0 ), then, as no tensile stress can
occur, no load can be taken:

wI = 0

Case II
We consider the same beam, but with centroidal axial prestress as shown:

P P
A B
C
L
VA VB

Now we have two separate sources of stress:

P MC P MC
+
A Zt A Zt

+
+ + =

P MC P MC

A Zb A Zb

20 P.Senapati
Prestressed Concrete
B.Tech,

For failure to occur, the moment caused by the load must induce a tensile stress
P
greater than . Hence, just prior to failure, we have:
A

M C P wL2
= =
Zb A 8Zb
8Z P
wII = b
L2 A

Note that we take Compression as positive and tension as negative.

Also, we will normally take Zb to be negative to simplify the signs.

Case III
In this case we place the prestress force at an eccentricity:

e e
P P
C
A B
L
VA VB

Using an equilibrium set of forces as shown, we now have three stresses acting on the
section:

e
N.A.
= P
P
M = Pe
21 P.Senapati
Prestressed Concrete
B.Tech,

Thus the stresses are:

P Pe MC P MC − Pe
+ Zt
A Zt Zt A Zt

+
+ + + =
+
P Pe MC P MC Pe
− +Z
A Zb Zb A Zb b

Hence, for failure we now have:

M C P Pe
= +
Zb A Zb
8Z  P Pe 
w = b +
L  A Z b 
2 
III

d
If, for example, we take e = , then:
6

P
8Zb  P
Pd 6  16Zb = 2  w
w = + =
III   II
L2 A bd 2 6 L2 A
 

So the introduction of a small eccentricity has doubled the allowable service load.

22 P.Senapati
Prestressed Concrete
B.Tech,

Numerical Example – No Eccentricity

Prestress force (at transfer), P = 2500 kN. Losses between transfer and SLS = 20%.
Check stresses. Permissible stresses are:
ftt = -1 N/mm2 ftc = 18 N/mm2
fst = 0 N/mm2 fsc = 22 N/mm2

The section is rectangular, 300 wide and 650 mm deep. It is simply supportedspanning
12 m with dead load equal to self weight and a live load of 6 kN/m (unfactored). The
prestress force is applied at the centroid.

First calculate the section properties for a 300650 beam:

x=h/2
A = 300650
= 195 000 mm2 h

Second moment of area, I, is bh3/12:

I = 3006503/12
= 6866106 mm4

Section modulus for the top fibre, Zt, is I/x. For a rectangular section 650 mm deep, the
centroid is at the centre and this is:

Zt = 6866106/325 = 21.12106 mm3

(some people use the formula for rectangular sections, Zt = bh2/6 which gives the same
answer).

23 P.Senapati
Prestressed Concrete
B.Tech,

Similarly, Zb = -21.12106 mm3 (sign convention: Zb is always negative as the


measurement to the bottom fibre is negative).

The only applied loading at transfer is the self weight which is (density of concrete) 
(area). Hence:

self weight = 25(0.3  0.65) = 4.88 kN/m

The maximum moment due to this loading is:

transfer moment, Mt = 4.88(12)2/8 = 87.8 kNm

wl2/8

The total loading at SLS is this plus the imposed loading, i.e.:

SLS moment, Ms = (4.88 + 6)(12)2/8


= 195.8 kNm

The prestress causes an axial stress of P/A = 2500103 / 195 000 = 12.8 N/mm2:

24 P.Senapati
Prestressed Concrete
B.Tech,

12.8

At transfer, the stress due to prestress applies and, after the beam is lifted, the stress
due to self weight. The self weight moment at the centre generates a top stress of:

Mt/Zt = 87.8106 / 21.12106 = 4.2 N/mm2.

Hence the transfer check at the centre is:

12.8 4.2 17.0 ✓

+ =

-4.2 8.6 ✓

Prestress Self Weight Total

At SLS, the prestress has reduced by 20%. The top and bottom stresses due to applied
load (Ms) are 195.8106/21.12106 = 9.3 N/mm2. Hence the SLS check is:

10.2 9.3 19.5 ✓

+ =

-9.3 0.9 ✓

Prestress Self Weight Total


25 P.Senapati
Prestressed Concrete
B.Tech,

Numerical Example – With Eccentricity

As per the previous example, but the prestress force is P = 1500 kN at 100 mm below
the centroid.

An eccentric force is equivalent to a force at the centroid plus a moment of force 


eccentricity:

P P
0.1m

This is equivalent to:

P P

0.1P 0.1P

Hence the distribution of stress due to prestress at transfer is made up of 2


components:
7.7
P/A = 1500103 / 195 000 = 7.7 N/mm2

7.7

26 P.Senapati
Prestressed Concrete
B.Tech,

(1500  103 )(100)


And + Pe/Z. At top fibre, this is - = -7.1
21.12 106

-7.1

+
7.1

As the moment is hog, the stress at the top is tension, i.e., negative. Similarly the
stress at the bottom fibre is +7.1

0.6
Hence the total distribution of stress due to PS is:

Hence the transfer check is: 14.8

0.6 4.2 4.8 ✓

+ =

14.8 -4.2 10.6 ✓

Prestress Dead Load Total

27 P.Senapati
Prestressed Concrete
B.Tech,

At SLS, the prestress has reduced by 20% (both the P/A and the Pe/Z components are
reduced by 20% as P has reduced by that amount). The stress distribution due to applied
load is as for Example 1. Hence the SLS check is:

0.48 9.3 9.8 ✓


+ =

11.8 -9.3
2.5 ✓

Prestress Applied load Total

28 P.Senapati
Prestressed Concrete
B.Tech,

3. Design of PSC Members

3.1 Basis

Sign Convention

In order to derive equations that enable design, we maintain a rigid sign convention:

• Moment:
Positive sag;
• Eccentricity of prestress:
Positive above centroid;
• Section Modulus:
Negative for the bottom of the member;
• Stress:
Positive compression.

With this sign convention, we now have:

P Pe MC
A Zt Zt t
+
+ + + =
+
P Pe MC b
A Zb Zb

Thus the final stresses are numerically given by:

29 P.Senapati
Prestressed Concrete
B.Tech,
P Pe MC
 = + +
Top fibre:
t
A Zt Zt
P Pe MC
Bottom fibre:  = + +
b
A Zb Zb

Note that the sign convention means that:


• the P A terms is always positive;

• the M C Z term is positive or negative depending on whether it is Zt or Zb ,

and;
• the Pe Z term is negative for Z t since Zt is positive and e is negative and the

term is positive for Zb since now both Zb and e are negative.

These signs of course match the above diagrams, as they should.

Governing Inequalities

Given the rigid sign convention and the allowable stresses in the concrete, and noting
that the losses are to be taken into account, the stresses are limited as:

Transfer
Top fibre – stress must be bigger than the minimum allowable tensile stress:

t  ftt
P Pe M t (1)
+ +  ftt
A Zt Zt

30 P.Senapati
Prestressed Concrete
B.Tech,
Bottom fibre – stress must be less than the maximum allowable compressive stress:

31 P.Senapati
Prestressed Concrete
B.Tech,

b  ftc
P Pe M t (2)
+ +  ftc
A Zb Zb

Service
Top fibre – stress must be less than the maximum allowable compressive stress:

t  fsc
 P Pe  M s (3)
 + +  f
  sc
A Zt  Zt

Bottom fibre – stress must be bigger than the minimum allowable tensile stress:

b  fst
 P Pe  M s (4)
 + +  f
  st
 A Z b  Zb

In these equations it must be remembered that numerically, any allowable tension is a


negative quantity. Therefore all permissible stresses must be greater than this allowable
tension, that is, ideally a positive number indicating the member is in compression at
the fibre under consideration. Similarly, all stresses must be less than the allowable
compressive stress.

32 P.Senapati
Prestressed Concrete
B.Tech,

3.2 Minimum Section Modulus


Given a blank piece of paper, it is difficult to check stresses. Therefore we use the
governing inequalities to help us calculate minimum section modulii for the expected
moments. This is the first step in the PSC design process.

Top Fibre
The top fibre stresses must meet the criteria of equations (1) and (3). Hence, from
equation (1):

P Pe Mt
+ +  ftt
A Zt Zt

P Pe  Mt   f
 + +
A Z  tt
 t 
Zt
  P Pe  
−   A + Z Mt
+   − ftt
  
t  Z t

If we now add this to equation (3):

  P Pe  M    P Pe  Mt 

  +  + s
− 
   +  +    f − f
A Z Z A Z Z sc tt

 t  t    t  t 

Ms Mt
−  f − f
sc tt
Zt Zt

Hence:

33 P.Senapati
Prestressed Concrete
B.Tech,

M −
t
 (5)
f sc tt

34 P.Senapati
Prestressed Concrete
B.Tech,

Bottom Fibre
The bottom fibre stresses must meet equations (2) and (4). Thus, from equation (2):

P Pe Mt
+ +  ftc
A Zb Zb

 P Pe 
+ t  f
M
 +
  tc
 A Z b  Z b
  P + Pe  
− A Z Mt
+   − ftc
  
b  Zb

Adding equation (4) to this:

  P Pe  M    P Pe  Mt 

  +  + s
− 
   +  +    f − f
A Z Z A Z Z st tc

 b  b    b  b 
Ms Mt
−  f − f
st tc
Zb Zb

Hence:

M −
 (6)
 ftc − fst
b

Note that in these developments the transfer moment is required. However, this is a
function of the self weight of the section which is unknown at this point. Therefore a
trial section or a reasonable self weight must be assumed initially and then checked
once a section has been decided upon giving the actual Zt and Zb values.

35 P.Senapati
Prestressed Concrete
B.Tech,

Example

Problem
The single-span, simply-supported beam shown below carried the loads as shown.
Taking the losses to be 25% and:
• permissible tensile stresses are 2.5 N/mm2 at transfer and 2.0 N/mm2 in
service;
• permissible compressive stresses are 20 N/mm2 at transfer and at service.
Determine an appropriate rectangular section for the member taking the density of
prestressed concrete to be 25 kN/m3.

Solution
We will check the requirements at the critical section which is at mid-span. To
determine an approximate initial transfer moment, M t , we estimate the section depth
based on a span depth ratio of, say, 15:

9000
d = = 600 mm
trial
15

Try this with a width of 250 mm, which is a practical minimum. Hence, the sefl
weight load is:
36 P.Senapati
Prestressed Concrete
B.Tech,

wsw = 25(0.6  0.25) = 3.75 kN/m

At transfer only self weight is present. Therefore:

wL2 3.75  92
Mt = = = 38 kNm
8 8

At service the moment is:

wL2 3.75 + 5 + 20 9 2

Ms = = = 291 kNm
8 8

Check the section modulus at the top fibre:

Ms −Mt
Zt 
f sc −  f tt
291 − 0.75  38
Zt 
20 − 0.75(−2.5)
Zt  12.0 106 mm3

And at the bottom:

M −M
Z b   sf − f t
tc st

291 − 0.75  38
Zb 
0.75(20) − (−2.0)
Zb  15.4 106 mm3

37 P.Senapati
Prestressed Concrete
B.Tech,
Z = Z and so the requirement for Zb
If the section is to be rectangular, then b t

governs:

bh 2
Z=  15.4 106
6

Keeping the 250 mm width:

250h2
 15.4 106
6

6 (15.4 106 )
h
250
h  609 mm

Thus adopt a 250 mm × 650 mm section.

Note that this changes the self weight and so the calculations need to be performed
again to verify that the section is adequate. However, the increase in self weight is
offset by the larger section depth and hence larger section modulii which helps reduce
stresses. These two effects just about cancel each other out.
Verify This

38 P.Senapati
Prestressed Concrete
B.Tech,

3.3 Prestressing Force & Eccentricity


Once the actual Zt and Zb have been determined, the next step is to determine what

combination of prestress force, P and eccentricity, e, to use at that section. Taking


each stress limit in turn:

Tensile Stress at Transfer

Taking the governing equation for tensile stress at transfer, equation (1), we have:

P Pe Mt
+ +  ftt
A Zt Zt
1
P + e Mt
f −
 A Z  tt
t  Zt
Zt
ftt − M t since e Z is negative
P

1 A + e Zt
t

1
 t

P ftt − M t Z t

Hence:

1  1 Zt 1A
   f −M Z 
P  ftt − M t Z t 
(7)
 tt t t 

This is a linear equation in 1 P and e. Therefore a plot of these two quantities will give
a region that is acceptable and a region that is not acceptable, according to the
inequality.

39 P.Senapati
Prestressed Concrete
B.Tech,

40 P.Senapati
Prestressed Concrete
B.Tech,

Compressive Stress at Transfer

Based on equation (2) which governs for compression at transfer, we have:

1
P + e  Mt
f −
 A Z  tc
b  Zb

Which leads to:

1  1A
  1 Zb
Z b  f Z b 
(8)
 ftc t  tc t

Another linear equation which gives the feasible region graphed as:

41 P.Senapati
Prestressed Concrete
B.Tech,

Compressive Stress in Service

Equation (3) governs for compression in service and so we have:

1
P + e Ms
f −
 A Z  sc
t  Zt

From which we get another linear equation in 1 P and e:

1   Zt  A

Z t   Z t 
(9)
 f sc s  f sc s

This equation can again be graphed to show the feasible region. However, this line can
have a positive or negative slope. When the slope is negative, 1 P must be under the
line; when the slope is positive, 1 P must be over the line. A simple way to
remember this is that the origin is always not feasible. Both possible graphs are:

42 P.Senapati
Prestressed Concrete
B.Tech,

43 P.Senapati
Prestressed Concrete
B.Tech,

Tensile Stress in Service

Lastly, we have equation (4) which governs for tension at the bottom fibre during
service. This gives:

1
P + e  Ms
f −
 A Z  st
b  Zb

Which gives:

1   Zb  A

Z b  f Z b 
(10)
f st  st

And this is graphed to show the feasible region:

44 P.Senapati
Prestressed Concrete
B.Tech,

Magnel Diagram

A Magnel Diagram is a plot of the four lines associated with the limits on stress. As
can be seen, when these four equations are plotted, a feasible region is found in which
points of 1 P and e simultaneously satisfy all four equations. Any such point then
satisfies all four stress limits.

Added to the basic diagram is the maximum possible eccentricity – governed by the
depth of the section minus cover and ordinary reinforcement – along with the
maximum and minimum allowable prestressing forces. For economy we usually try
to use a prestressing force close to the minimum.

The geometric quantities Zt A and Zb A are known as the upper and lower kerns

respectively. They will feature in laying out the tendons.

45 P.Senapati
Prestressed Concrete
B.Tech,

Example

Problem
A beam, 200 mm wide × 350 mm deep spans 10 m and carries 3 kN/m live load in
addition to its dead weight. The concrete is grade 40 and the prestress is transferred at
32 N/mm2 cube strength. Take prestress losses to be 20%. The member is to be a Class
1 member.

Draw the Magnel diagram for the mid-span section and determine an economic
prestressing force and its corresponding eccentricity.

Solution
The self weight is:
wsw = 25(0.2  0.35) = 1.75 kN/m

The section properties are:

A = bh = 200  350 = 70 103 mm2

bh2 200  3502


Zt = Z b = = = 4.083106 mm3
6 6

At transfer only self weight is present. Therefore:

wL2 1.75 102


Mt = = = 21.9 kNm
8 8

At service the moment is:


46 P.Senapati
Prestressed Concrete
B.Tech,
wL2 1.75 + 3 10 2

Ms = = = 59.4 kNm
8 8

The allowable stresses are, for a Class 1 member, from the previous table:

ftt = −1 N/mm2 f tc = 0.5  32 = 16 N/mm2


f st = 0 N/mm2 f sc = 0.33 40 = 13.33 N/mm2

Next we determine the equations of the four lines:

• ftt : The denominator stress is:

 tt = f tt − M t Z t = −1 − 21.9 4.083 = −6.37 N/mm2

Hence:

1 1 4.083106  1 70 103 

P 

−6.37  e +  −6.37 
 
106
 −0.0385e − 2.243
P

• ftc : The denominator stress is:

 tc = ftc − M t Z b = 16 − 21.9 −4.083 = 21.37 N/mm2

47 P.Senapati
Prestressed Concrete
B.Tech,
Hence:

48 P.Senapati
Prestressed Concrete
B.Tech,
1 1 −4.083106  1 70 103 

P 

21.37  e +  21.37 
 
106
 −0.0115e + 0.668
P

• ftc : The denominator stress is:

 sc = f sc − M s Z t = 13.33 − 59.4 4.083 = −1.24 N/mm2

Hence:
1  0.8 4.083106   0.8 70 103 

 −1.24 e +  −1.24 
P    
106
 −0.158e − 9.21
P

• fst : The denominator stress is:

 st = f st − M s Z b = 0 − 59.4 −4.083 = 14.57 N/mm2

Hence:

1  0.8 −4.083106   0.8 70 103 



 14.57 e +  
P  14.57 
 
106
 −0.00135e + 0.784
P

49 P.Senapati
Prestressed Concrete
B.Tech,

Notice that the 106 has been brought to the left so that we are working with larger

numbers on the right hand sides. To plot these lines, note that the vertical intercepts
are known and the x-axis values are also known to be:

50 P.Senapati
Prestressed Concrete
B.Tech,

−Z t −4.083106
= = −58.33 mm
A 70 103

−Z b − ( −4.083106 )
= = +58.33 mm
A 70 10 3

We plot the lines using these sets of points on each of the axes:
ftt

106/P (106/N)
10 ftc
fsc
8
fst
6

0
-150 -100 -50 0 50 100 150
-2
Eccentricity (mm)
-4

-6

-8

-10

For clarity in these notes, we zoom into the area of interest:

51 P.Senapati
Prestressed Concrete
B.Tech,

ftt

106/P (106/N)
3 ftc
fsc
fst
2.5

1.5

0.5
Eccentricity (mm)
0
-150 -100 -50 0 50 100 150

So from this figure, the minimum prestressing is the highest point in the region (or
maximum y-axis value) permissible, which is about 2.4. Hence:

106
= 2.4
P
106
P=
2.4
= 416 103 N
= 416 kN

The corresponding eccentricity is about 120 mm below the centroidal axis.

Obviously these values can be worked out algebraically, however such exactitude is
not necessary as prestress can only be applied in multiples of tendon force and
eccentricities are to the nearest 10 mm practically.

52 P.Senapati
Prestressed Concrete
B.Tech,

3.4 Eccentricity Limits and Tendon Profile


Up to now we have only considered the critical location as defined by the position of
the maximum moment: the mid-span of the simply supported beam. However, the
governing inequalities (i.e. the stress limits) must apply at every section along the
beam.

Thus far we have established an appropriate section and chosen a value for P, which
remains essentially constant along the length of the span. We have also found a value
for the eccentricity at the critical location.

Since the moments change along the length of a beam, we must change some aspect of
the prestress also. The only remaining variable is the eccentricity. As we wish to limit
possible tensile stresses, we only examine equations (1) and (4) correspondingto
tension on the top at transfer and tension on the bottom in service.

Tension on Top at Transfer


We determine an expression for the eccentricity in terms of the other knowns:

P Pe Mt
+ +  ftt
A Zt Zt
Zt ftt  Zt M t 
e  
P − A+ P
 

Hence we have a lower limit for the eccentricity as:

Zt Zt ftt − M t
elower  − + (11)
A P

53 P.Senapati
Prestressed Concrete
B.Tech,

Tension on the Bottom in Service


Using equation (4):

 P Pe  M s
 + +  f st
 A Z b  Zb

e  b st −  Zb + M s 
Zf
P A P 

 

Hence we have an upper limit for the eccentricity as:

Zb Zb fst − M s
eupper  − + (12)
A P

Since the upper and lower kerns (the Zt A and Zb A quantities) are constant for

constant geometry, and since P is also constant, it can be seen that the cable limits
follow the same profile as the bending moment diagrams at transfer and in service.

54 P.Senapati
Prestressed Concrete
B.Tech,

Example

Problem
For the beam of the previous example, sketch the upper and lower eccentricities
given a prestress of 450 kN.

Solution
In the previous example, the kerns were found to be

−Z t
= −58.33 mm
A
−Zb = +58.33 mm
A

The ‘tension moments’ are:

M tt = Z t f tt = ( 4.083106 ) ( −1) = −4.083 kNm


M st = Z b f st = ( −4.083106 ) ( 0 ) = 0 kNm

Hence for the lower limit we have:

=−
Zt Zt ftt − M t
e +
lower
A P
−4.083 − M t , x
= −58.33 +
450
M
= −58.33 −1.02 − t , x
450
M
= −59.35 − t ,x
450

55 P.Senapati
Prestressed Concrete
B.Tech,

And for the upper:

Zb Zb fst − M s
eupper = − +
A P
0−M
= 58.33 + s,x

0.8  450
M
= 58.33 − s , x
360

Knowing the values of the bending moments at positions along the beam, we can now
plot the eccentricity limits:

centroid low er upper


250
Distance from Soffit (mm)

200

150

100

50

0
0.00 2.00 4.00 6.00 8.00 10.00
Distance Along Beam (m)

In this figure the upper and lower eccentricities are very close at the critical section.
This is because the chosen prestress is very close to the minimum possible from the
permissible region. A higher prestress would give ‘looser’ limits.

56 P.Senapati
Prestressed Concrete
B.Tech,

Debonding

Notice from the eccentricity limits of the previous example that a straight cable/tendon
profile will not work. Yet we know from the discussion on factory precasting of
prestressed sections that straight tendons are preferable.

By changing the prestress force along the length of the beam, we can find a solution
to this problem. From the previous example the new eccentricity limits are:

centroid low er upper Straight Profile


250

200
Distance from Soffit (mm)

150

100

50

0
0.00 2.00 4.00 6.00 8.00 10.00
Distance Along Beam (m)

It can be seen that an eccentricity of 85 mm below the centroidal axis works.

Note that it appears that there remains a problem at the ends of the beam. However, the
cable force gradually increases in reality due to the transmission zone (i.e. the bond
between the tendon and concrete). Hence the stresses will be acceptable in this zone
also.

57 P.Senapati
Prestressed Concrete
B.Tech,

The straight profile required the following variation of prestress:

700

600

500
Prestress (kN)

400

300

200

100

0
0.00 2.00 4.00 6.00 8.00 10.00
Distance Along Beam (m)

Note that the maximum prestress has been increased from 450 kN to 600 kN. Even
thought he extra strand is an added expense; it is offset by the constructability of the
member.

Note that the prestress steps up in units of 200 kN at two points. Imagine there to be 3
tendons acting, each of 200 kN prestress:
• From 0 to 1.5 m only 1 tendon is to act;
• From 1.5 to 3 m 2 tendons are to act;
• From 3 to 5 m all 3 tendons are to act
(Note that the prestress is symmetrical.)

58 P.Senapati
Prestressed Concrete
B.Tech,

In a factory setting, all 3 tendons will be present and yet some are not to act.
Therefore the bond between the concrete and tendon is broken by using plastic tubing
over the required length. Hence for our beam, the layout will look like:

(Note this is slightly unrealistic as vertical symmetry is maintained in reality.)

Briefly then for post-tensioned members in general, the section properties, the
bending moments, and the prestress all may change along the length of a member:

Mt and Ms
Mt and Ms
Hogging
Sagging
Mt = Ms = 0

In such beams, the governing stress limits must be checked at ‘every’ point along the
length of the beam.

59 P.Senapati
Prestressed Concrete
B.Tech,

4. Prestressing Losses

4.1 Basis and Notation


Recall that transfer is the moment at which the concrete first feels the prestress.
Losses can be before or after transfer:
• Before-transfer losses are the difference between what is applied by the hydraulic
jack, Pjack and what the concrete feels at transfer, Pt ;

• After-transfer losses are the difference between the transfer force, P and the force
at SLS, P =  P .
s t

The calculation of losses is different for pre- and post-tensioned PSC.

Notation

fp = prestress in strand or tendon;

Ap = cross-sectional area of prestressing tendon;

Ep = modulus of elasticity (Young's modulus) of prestressing steel;

Ec = modulus of elasticity (Young's modulus) of concrete;


Ag = gross cross-sectional area of concrete member;

Ig = gross second moment of area of concrete member;

P = prestress force at transfer;


Pjack = prestress force applied by jack (prior to before-transfer losses);

fc = stress in concrete;

 = strain;
 sh = strain in concrete due to shrinkage;
 = creep strain in concrete an infinite time after prestressing at SLS;
60 P.Senapati
Prestressed Concrete
B.Tech,
 = creep strain per unit of sustained stress.

61 P.Senapati
Prestressed Concrete
B.Tech,

4.2 Losses in Pre-Tensioned PSC

1. Elastic Shortening Loss

In pre-tensioning, the strands are stressed before the concrete is cast. Therefore, after
jacking ( Pjack ) has been applied, at a level y, the concrete is subjected to the stress:

Pjack ( P e) y
jack M y
fc, y = + + o

Ag Ig Ig

At the level of the strands, y = e . Hence, the stress in the concrete at that level is:

P P e2 Me
f c,e = jack
+ jack
+ o

Ag Ig Ig

And the concrete at the level of the strands has a strain of:

fc,e
 c,e =
Ec

Since the strands are bonded to the concrete, they undergo a loss of strain of the same
amount,  c,e , with associated stress and force losses of E p c,e and Ap E p c,e . Hence:

AE P P e2 M e
P = E
 A + I + It 
p p jack jack

c  g g g 

The concrete never feels the full jacking force since the strands shorten as the

62 P.Senapati
Prestressed Concrete
B.Tech,
concrete strains. Hence, elastic shortening loss in pre-tensioning is ‘before-transfer’.

63 P.Senapati
Prestressed Concrete
B.Tech,

2. Shrinkage Loss

Concrete shrinks as it sets and for a period afterwards. The amount of shrinkage
depends on the humidity and the surface area to volume ratio. Once again, as the strands
are bonded to the concrete they undergo the same strain. Hence the loss of prestress is:

P = A E 
sh p p sh

Shrinkage loss is long-term. Hence it is ‘after-transfer’.

3. Relaxation Loss

When maintained at a constant strain, prestressing strand gradually loses its stress with
time (like a guitar going out of tune). It is due to a realignment of the steel fibres and is
the same phenomenon as creep. Depending on the quality of the steel, relaxation losses
can vary in the range of 3% to 8%.

Stress
 = constant

time

Relaxation is ‘after-transfer’.

64 P.Senapati
Prestressed Concrete
B.Tech,

4. Creep Loss

Creep is the ongoing increase in strain with time, when stress is kept constant:

Strain

 = constant

time

Creep causes a strain in the concrete adjacent to the strands and over a long time is:

  =  f c,e

The creep factor  depends on a number of things such as concrete quality and its
age when loaded. Thus the strands slacken as before, and the loss of force is:

P =AE
creep p p 

= Ap E p f c,e
  P  Pe 2 M e 
= A E  t + t + perm

p p
 Ag Ig I g 

M perm is the moment due to the permanent loads such as the prestress, dead load and

superimposed dead loads such as such as parapets and road pavement). As creep loss
contributes to  , an exact calculation is iterative. Creep is long term, hence it is an
‘after-transfer’ loss.

65 P.Senapati
Prestressed Concrete
B.Tech,

4.3 Losses in Post-tensioned PSC

1. Elastic Shortening Loss

This loss only occurs in post-tensioning when there is more than one tendon.

Two Tendons
As a simple example, take the following beam with two tendons:

Tendon 1 is stressed first. The operator applies prestress until the gauge indicates the
required prestress force is applied. The beam shortens during this process but this is
compensated for, as it is jacked until the required prestress force is applied. Hence there
is no elastic shortening loss to be allowed for at this stage.

Tendon 1 is anchored and Tendon 2 is stressed. This causes strain at the level of Tendon
1, resulting in a prestress loss in Tendon 1. The stress due to Tendon 2 is:

P2 ( P2e2 ) y
fc ,2 = +
Ag Ig

Note that the actual properties are approximated with the gross properties, Ag and I g .

The strain due to the stressing of Tendon 2, in the concrete adjacent to Tendon 1, is:
66 P.Senapati
Prestressed Concrete
B.Tech,

1  P ( P2e2 ) e1 
 c,2 = +
 2
Ec  Ag I g 

This is the amount of strain lost in Tendon 1. Hence the loss of prestress force is:

P = Ap1 E p P + ( P2 e2 ) e1
 
2  2 
Ec  Ag Ig 

The stressing of Tendon 2 does not cause any losses in Tendon 2 – it only causes
losses in tendons that have already been anchored.

Multiple Tendons
Similar calculations can be made for any arrangement of tendons. For 4 tendons:
1. stressing the first tendon does not cause any losses;
2. stressing the 2nd causes a loss in the 1st;
3. stressing the 3rd causes losses in the 1st and 2nd;
4. stressing the 4th causes losses in the 1st, 2nd and 3rd.

Hence the first tendon has losses due to the stressing of Tendons 2, 3 and 4, the
second due to the stressing of 3 and 4 and the third due to the stressing of 4 giving:

P = Ap1Ep  P + P + P + ( P2e2 + P3e3 + P4e4 ) e1  + Ap 2 E p P + P


+
(Pe
3 3 + P4e4 ) e2 

  
3 4


2 3 4
2−4
Ec  Ag Ig  Ec  Ag Ig 

Ap 3 E p  P ( P4e4 ) e3 
+ +
 4 
Ec  Ag Ig 

Elastic shortening loss is ‘before-transfer’.


67 P.Senapati
Prestressed Concrete
B.Tech,

2. Shrinkage Loss

Calculation is as for pre-tensioned PSC and is an ‘after-transfer’ loss.

3. Relaxation Loss

Calculation is as for pre-tensioned PSC and is an ‘after-transfer’ loss.

4. Creep Loss

Calculation is as for pre-tensioned PSC and is an ‘after-transfer’ loss.

5. Friction Curvature Loss

When the jacking force is applied, there is a friction between the tendon and the duct
that prevents the interior parts of the beam/slab from feeling the full force:

‘live’ dead end


friction
anchor anchor

Pjack

Examining a portion of the tendon, the loss is:

P = P −P
fric jack l

= Pjack (1 − e−  )

68 P.Senapati
Prestressed Concrete
B.Tech,

where  is the aggregate change in angle from the jack (in radians) (the sum of the
absolute values of each change in angle) and  is the roughness (friction) coefficient.

Pjack

P1 = Pjacke -

Example (jacked from left only)

Dead
Jack
Anchor
2 C
Pjack
1 3
A B

At A: loss = Pjack (1 − e−  ) 1

At B: loss = Pjack (1 − e−  ( + ) )
1 2

At C: loss = Pjack (1 − e−  ( + + ) )
1 2 3

where 1 + 2 + 3 is the aggregate change in angle from Pjack, regardless of sign.

Friction curvature loss happens between the jack and a-section. Therefore the section
never feels the full jacking force and this loss is ‘before transfer’.

69 P.Senapati
Prestressed Concrete
B.Tech,

6. Friction Wobble Loss

This loss is due to ‘unintentional variation of the duct from the prescribed profile’:

wobbly duct

tendon

friction

This loss increases with distance from the jack and is given by:

P =P (1 − e )
− kx

wobble jack

where x = distance from jack, and k is a wobble coefficient (function of workmanship,


distance between duct supports, stiffness of duct, etc.). This is a ‘before transfer’ loss.

70 P.Senapati
Prestressed Concrete
B.Tech,

7. Draw-In Loss

Anchors consist of wedges that ‘draw in’ when the jack ceases to be applied:

wedges wedge
draw in

strand

Jack

During stressing After jack is

The draw in of the wedges can be up to 10 mm but the loss is generally local:

Force
Friction losses
Pjack (curvature + wobble)

Draw in Prestress force after


friction and draw in
losses
Distance from live anchor

Draw in losses are not transmitted more than about 5-10 m from the live anchor.
Formulas are available which give the extent and magnitude of the draw in loss.

There is some debate about whether draw in should be considered to be ‘before-


transfer’ or ‘after-Transfer’ but it is safer to take it to be an ‘after-transfer’ loss.

71 P.Senapati
Prestressed Concrete
B.Tech,

5. Ultimate Limit State Design of PSC

5.1 Ultimate Moment Capacity


The ULS moment capacity of a PSC section is calculated using the assumption that
plane sections remain plane. This is similar to the approach for ordinary reinforced
concrete. There is one difference:
• the strain in bonded prestress steel is equal to the strain caused by the initial
prestress plus the change in strain in the concrete at the prestressing steel level.

The following diagram shows the strain diagram at three stages of loading:

Stage 1
This is the strain diagram at transfer. The strain in the concrete at steel level is
compressive, with magnitude of:

1
 =  Pt Pe2 
+
E A I 
ct

c  

72 P.Senapati
Prestressed Concrete
B.Tech,

The stress and strain in the prestressing steel are:

f
f pt = Pt  pt = Ept
A
p p

Stage 2
The applied moment is sufficient to decompress the concrete at the steel level.Provided
there is a bond between the steel and concrete, the change in strain in the prestressing
steel is equal to that of the concrete at the steel level. Hence the strain in the prestressing
steel is now  +  . pt ct

Stage 3
This is the strain diagram at the ultimate load. The concrete strain at the steel level,
 cpu , is related to the concrete strain at the top of the section by similar triangles:

 =   dp − x 
cu 
x 
cpu

 

The change in strain in the prestressing steel is, by compatibility, the same as  cpu .

Final
The final strain in the prestressing steel at ultimate load is thus:

 pu =  pt +  ct +  cpu

In this equation, it is only  cpu that is not known. This can be obtained once a depth of

neutral axis is found that balances horizontal forces.


73 P.Senapati
Prestressed Concrete
B.Tech,

Example

Problem
Determine the ultimate moment capacity of the section shown. The steel tendon has a
transfer prestress of 1200 kN and the area of the strand is 1000 mm 2. The elastic
modulus for the prestressing steel is 195 kN/mm2 and the concrete is 45 N.

350 0.45fcu
cu

Fc
x
750 650 s = 0.9x

Ap
cpu Pu

Beam Strain Stress/Force


Section Diagram Diagram

Solution
The initial strain in the tendon due to the prestress is:

 =
P
= 1200 103
t
= 0.00615
pt
Ep Ap (195 103 )(1000)

The strain in the concrete caused by the initial prestress is:

1
 =  Pt Pe2 
+
E A I 
ct

c  
1  1200 103
= 
74 P.Senapati
Prestressed Concrete
B.Tech,

(1200 10 ) ( 275)


3 2

29.8 103  750  350 + 
350  7503 12
 
= 0.00040

75 P.Senapati
Prestressed Concrete
B.Tech,

At failure, the concrete strain at the level of the prestressing is:

 650 − x 
 cpu = 0.0035 
x 
 

And so the final strain in the prestressing steel is:

 650 − x 
 pu = 0.00655 + 0.0035
x 
 

And the final force in the prestressing steel is:

P =AE
  650 − x 
u p p pu

= (1000)(195 103 ) 0.00655 + 0.0035


  x 
  
6   650 − x 
= 195  + 0.0035
10 0.00655  x 
  

The force in the concrete is:

Fc = (0.45  45)(350  0.9x)


= 6379x

At the correct depth to the neutral axis we will have horizontal equilibrium of forces,
Pu = Fc . Hence we iteratively try to find this value of x:

76 P.Senapati
Prestressed Concrete
B.Tech,

x Fc Pu Difference

350 2232563 1862250 370312.5

250 1594688 2369250 -774563

300 1913625 2073500 -159875

315 2009306 2003083 6222.917

314 2002928 2007568 -4640.97

314.4 2005479 2005771 -291.992

Hence the moment capacity is:

M u = P uz
= Pu ( d p − 0.45x )
= 2005771 (650 − 0.45  314.4)
= 1020 kNm

77 P.Senapati
Prestressed Concrete
B.Tech,

5.2 Ultimate Shear Design

Background

The shear design procedure for PSC is quite different from ordinary RC. It varies
significantly from code to code. However, there is one issue with PSC that can have a
significant influence on shear design. This is the vertical component of the prestress
force which can have a significant beneficial effect.


P sin
P
P

Bearing

Also, the shear capacity depends on whether or not the section has cracked under the
ultimate flexural moments at the section.

Note that nominal links are required in PSC members, similarly to ordinary
reinforced members.

78 P.Senapati
Prestressed Concrete
B.Tech,

Shear Capacity for Cracked Sections

A section is cracked in flexure if the moment is greater than a design cracking


moment, M 0 , defined below. The cracked shear capacity, Vcr , is empirically give by:


V = 1 − 0.55 f ps  v b d + M o V  0.1b d
fcu
f  c v M
cr  v

 pu 

In which:
M is the moment acting at the section;
V is the shear acting at the section;
M0 is the moment required to remove 0.8 of the compressive stress at the level of
the prestress:
I
M 0 = 0.8 f c,e
e
where:

Ps Pe 2
fc,e = + s

Ag Ig
f ps is the stress in the tendon at SLS;

f pu
is the ultimate tensile strength of the tendon;

bv is the shear width of the web/section;

d is the effective depth;


vc is the design shear strength of the concrete:

v = 0.79  100 As   400  0.25  f 0.33


0.33
cu
  
1.25  bv d   d   25 
c

79 P.Senapati
Prestressed Concrete
B.Tech,

Shear Capacity for Uncracked Sections

A section is uncracked if the applied moment is less than M 0 . In such section, the

fcu
principal tensile stress in the web is limited to f t = 0.24 . Based on a Mohr’s

circle analysis, the following equation is derived:

f t 2 + 0.8 ft fcp
Vco = 0.67bh +V
p

In which:
fcp is the compressive stress due to prestress at the centroidal axis:

Ps
fcp =
A

Vp is the vertical component of prestress at the section, resisting the applied shear;

And the remaining variables have their previous meaning.

80 P.Senapati
Prestressed Concrete
B.Tech,

Shear Design

The design shear resistance at a section is:

Uncracked: Vc = Vco
Cracked: Vc = min Vco ,Vcr 

The shear design is:


• V  0.5Vc : no links are required;
• V  V + 0.4b d : Shear links are used:
c v

Asv 0.4bv
=
sv 0.87 f yv

• V  V + 0.4b d : Shear links are used:


c v

Asv V − Vc
=
sv 0.87 f yvdt

Where:
Asv is the link area;
sv is the link spacing;
f yv is the characteristic strength of the links;

dt is the depth to the furthest steel, ordinary or prestressed, from the compression
face.

81 P.Senapati
Prestressed Concrete
B.Tech,

Example

Problem
A Y-beam, as shown, has rib width of 200 mm and a depth of 1000
mm. Its area is 310 × 103 mm2 and its second moment of area is 36 ×
109 mm4. The area of prestressing steel is 1803 mm 2 which has
strength of 1750 N/mm2 and is stressed to 60% of its strength in
service at an eccentricity of 290 mm. The concrete is grade 50.

Check the section for a shear of 400 kN and associated moment of


800 kNm. Note that the tendon is inclined by 3˚ at the section
considered.

Solution
First determine the following:

Pt = Ap fs = (1803)(0.6 1750) = 1893 kN


Ps 1893103
f = = = 6.1 N/mm2
310 103
cp
A
ft = 0.24 fcu = 0.24 50 = 1.7 N/mm 2

Uncracked shear capacity:

Vco = 0.67bh f t 2 + 0.8 f t f cp + V p

= 0.67(200 1000) 1.7 2 + 0.81.7  6.1 + 1893sin 3∘


= 448.2 + 99.1
= 547.3 kN

82 P.Senapati
Prestressed Concrete
B.Tech,

For the cracked shear capacity, we have the following inputs:

f ps
= 0.6 given
f pu
2
Ps Pe
fc,e = + s

Ag Ig
1893103 (189310 ) ( 290 )
3 2

= +
310 103 36 109

= 10.52 N/mm2
I
M 0 = 0.8 f c,e
e
=  36 109 
0.8(10.52) 290 
 
= 1046 kNm
0.79  100 A 0.33 400 0.25 f 0.33
   
v = 
s
  cu
  
1.25  bvd   d   25 
c

0.79  100 1803   400   50 


0.33 0.25 0.33

=
1.25  200  790   790   25 
   
= 0.78 N/mm2

Hence:

V = 1 − 0.55 f ps  v b d + M o V  0.1b d
fcu
f  c v M
cr  v

 pu 

(400 103 )  0.1(200  790) 50


1046
= (1 − 0.55  0.6)(0.78  200  790) +
800
= 605.4  111.7
= 605.4 kN

83 P.Senapati
Prestressed Concrete
B.Tech,

The section is uncracked since M  M and so the design shear strength is 547.3 kN
0

which is greater than the applied 400 kN. Therefore, use nominal links.

84 P.Senapati