We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF or read online on Scribd
You are on page 1/ 1
WELD PROCEDURE
Date 25/08/2009
2 SPECIFICATION (WPS) | wos xo. :p02
= ACCORDING TO ASME IX |"
Sheet Loft
CONTRACTOR / OWNER. TECHINT / METHANEX”
‘WELDING PROCEDURE SPECIFICATION No. P02)
SUPPORTING PQR NO. P-8\8-T-12
PROCESS GTAW
‘TYPES ( Manual , Automatic, Semi Auto.) MANUAL
[sorts DESIGN
ik
BASE METAL,
Material Spee. A312
‘Type or Grade ‘TP304 — TP 304L
PINo.
Group No.
Thickness
Diameter
Other “Thickness Range Qualified
From $To 1am
FILLER METALS.
As
22-20mm
Weld Metal Analysis A No.
Size of Electrode
POSTWELD HEAT TREATMENT
‘Temperature Range ENA
‘Time Range NA
Other NA
‘Type of Gas or Gases Argon
Composition of Gas Mixture: 9.99%,
Other flow rate :6-201ivmin—
Backing Gas NAL
ELECTRICAL CHARACTERISTICS
Current :DC
Polarity Electrode -ve & +ve
Tungsten Electrode Type &Size _ :2.4 mm-EWTH 2%
FNo. F6 WELD [FILLER METAL CURRENT [vOut] Hear
SFA Specification AS98522 Thver [Cass] Diam [Pola [ama] RANGE | IN
‘AWS Classification ER3OSL (TGX) — (om) | "| sange aint
ER 308L, TT aR [2.2 [ave | 75-100 [10 [119
Weld Metal Deposit : 2 _[ersost_[ 2.0 |-ve | 75-100_[ 22-28 [1263
“Grove: >AW I mm 37 —[ersosc [2.0 [-ve [75-100 | 29-98 1247
= Fillet: ALL
POSITION
CaP _[ eRSORL | 30 [ve [75-100[ 23-28 987
Position of Groove 2 ALL TECHNIQUE
‘Weld Progression + Up bl for vertical idepan Cumailg Grinding & Wire
Other None iesh
PREHEAT String or Weave Bead ‘BOTH
Orifice oF Gas Cup Size 9-16 mm
Preheat Temp. (°C)( Min): Ambient Temp. Multipass or Single Pass Multi passes
Interpass Temp. (*C)( Max): 150°C Max Single or Multiple Electrodes: single
Other None Method Of Back gouging None
Peening None
JOB TITLE PTI QA/QCENG. ay @A/0C 7
‘NAME EHAB HOSSIN A.V p N
DATE 25/08/2009 u g.
SIGN. Gress %