0% found this document useful (0 votes)
226 views43 pages

دليل معمل هندسة الطرق والمطارات

The document provides an overview of the laboratory tests conducted at the Highway and Airport Engineering Laboratory (H&AE LAB) at Mansoura University. It outlines the various tests performed on aggregate materials, binders, unbound pavement layers and asphalt mixtures. Tests are conducted to determine key material properties like gradation, density, moisture content and strength. The document also lists the equipment used to perform the laboratory tests and provides templates for recording test results.

Uploaded by

husham ali
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
0% found this document useful (0 votes)
226 views43 pages

دليل معمل هندسة الطرق والمطارات

The document provides an overview of the laboratory tests conducted at the Highway and Airport Engineering Laboratory (H&AE LAB) at Mansoura University. It outlines the various tests performed on aggregate materials, binders, unbound pavement layers and asphalt mixtures. Tests are conducted to determine key material properties like gradation, density, moisture content and strength. The document also lists the equipment used to perform the laboratory tests and provides templates for recording test results.

Uploaded by

husham ali
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
You are on page 1/ 43

‫‪Mansoura University‬‬ ‫ﺟﺎﻣﻌــﺔ ﺍﻟﻤﻨﺼــﻮﺭﺓ‬

‫‪Faculty of Engineering‬‬ ‫ﻛﻠﻴـــــﺔ ﺍﻟﻬﻨﺪﺳــــــــﺔ‬


‫‪Center of Tech., Exp.,&Sci. Center Services‬‬ ‫ﻣﺮﻛﺰ ﺍﻟﺨﺪﻣﺎﺕ ﺍﻟﻔﻨﻴﺔ ﻭﺍﻟﻤﻌﻤﻠﻴﺔ ﻭﺍﻟﻌﻠﻤﻴﺔ‬
‫‪Highway and Airport Engineering Laboratory‬‬ ‫ﻣﻌﻤﻞ ﻫﻨﺪﺳﺔ ﺍﻟﻄﺮﻕ ﻭﺍﻟﻤﻄﺎﺭﺍﺕ‬
‫)‪(H&AE LAB‬‬

‫ﺩﻟﻴﻞ ﻣﻌﻤﻞ ﻫﻨﺪﺳﺔ ﺍﻟﻄﺮﻕ ﻭﺍﻟﻤﻄﺎﺭﺍﺕ‬


‫‪ ‬‬

‫ﻣﻠﺨﺺ ﺍﺟﺮﺍء ﺍﻟﺘﺠﺎﺭﺏ‬


‫‪ ‬‬
‫ﺟﺪﻭﻝ ﺍﻟﻤﺤﺘﻮﻳﺎﺕ‬
‫ﺍﻭﻻ‪ :‬ﺑﻴﺎﻧﺎﺕ ﺍﺟﻬﺰﻩ ﺍﻟﻤﻌﻤﻞ ﺍﻟﻤﺴﺘﺨﺪﻣﻪ ﻓﻲ ﺍﻟﺘﺠﺎﺭﺏ‪.‬‬
‫ﺛﺎﻧﻴﺎ‪ :‬ﺍﻟﺘﺠﺎﺭﺏ ﺍﻟﻤﻌﻤﻠﻴﺔ ﻟﻼﺣﺠﺎﺭ ﺍﻟﺼﻠﺒﻪ )ﺍﻟﺮﻛﺎﻡ(‪.‬‬
‫‪ -١‬ﺍﻟﺘﺪﺭﺝ ﺍﻟﺤﺒﻴﺒﻲ ﻟﻠﺮﻛﺎﻡ ﺍﻟﺨﺸﻦ ﺑﺎﺳﺘﺨﺪﺍﻡ ﺍﻟﻤﻨﺎﺧﻞ‪.‬‬
‫‪ -٢‬ﺍﻟﻮﺯﻥ ﺍﻟﻨﻮﻋﻲ ﻭﻧﺴﺒﻪ ﺍﻻﻣﺘﺼﺎﺹ ﻟﻠﺮﻛﺎﻡ ﺍﻟﺨﺸﻦ‪  .‬‬
‫‪ -٣‬ﺍﻟﻮﺯﻥ ﺍﻟﻨﻮﻋﻲ ﻭﻧﺴﺒﻪ ﺍﻻﻣﺘﺼﺎﺹ ﻟﻠﺮﻛﺎﻡ ﺍﻟﻨﺎﻋﻢ‪  .‬‬
‫‪ -٤‬ﺍﺧﺘﺒﺎﺭ ﻟﻮﺱ ﺍﻧﺠﻠﻮﺱ‪  .‬‬
‫‪ -٥‬ﺍﺧﺘﺒﺎﺭ ﺍﻟﻤﻜﺎﻓﺊ ﺍﻟﺮﻣﻠﻲ ﻟﻠﺘﺮﺑﻪ ﺍﻟﻨﺎﻋﻤﻪ‪.‬‬
‫‪ -٦‬ﺍﺧﺘﺒﺎﺭ ﻣﻘﺎﻭﻣﻪ ﺍﻟﺮﻛﺎﻡ ﻟﻠﺘﺎﻛﻞ )ﺑﺎﺳﺘﺨﺪﺍﻡ ﻣﺤﻠﻮﻝ ﻛﺒﺮﻳﺘﺎﺕ ﺍﻟﺼﻮﺩﻳﻮﻡ ﺍﻭ ﻛﺒﺮﻳﺘﺎﺕ ﺍﻟﻤﺎﻏﻨﺴﻴﻮﻡ(‪.‬‬
‫‪ -٧‬ﺍﺧﺘﺒﺎﺭ ﺣﺪﻭﺩ ﺍﻻﺗﺮﺑﺮﺝ ﻟﻠﻤﻮﺍﺩ ﺍﻟﻨﺎﻋﻤﻪ‪.‬‬
‫ﺛﺎﻟﺜﺎ‪ :‬ﺍﻟﺘﺠﺎﺭﺏ ﺍﻟﻤﻌﻤﻠﻴﺔ ﻟﻠﻤﺎﺩﻩ ﺍﻟﺮﺍﺑﻄﻪ )ﺍﻟﺒﺘﻮﻣﻴﻦ(‪.‬‬
‫‪ -١‬ﺍﺧﺘﺒﺎﺭ ﺍﻻﺧﺘﺮﺍﺝ ﻟﻠﺒﺘﻮﻣﻴﻦ‪  .‬‬
‫‪ -٢‬ﺍﺧﺘﺒﺎﺭ ﺍﻟﻠﺰﻭﺟﻪ ﺑﺎﺳﺘﺨﺪﺍﻡ ﻣﻘﻴﺎﺱ ﺍﻟﻠﺰﻭﺟﻪ ﺍﻟﺪﻭﺍﺭ‪  .‬‬
‫‪ -٣‬ﺍﺧﺘﺒﺎﺭ ﺍﻟﻜﺮﻩ ﻭﺍﻟﺤﻠﻘﻪ‪  .‬‬
‫ﺭﺍﺑﻌﺎ‪ :‬ﺍﻟﺘﺠﺎﺭﺏ ﺍﻟﻤﻌﻤﻠﻴﻪ ﻟﻄﺒﻘﺎﺕ ﺍﻟﻤﻔﻜﻜﻪ )ﺍﻻﺳﺎﺱ‪ ،‬ﺍﻻﺳﺎﺱ ﺍﻟﻤﺴﺎﻋﺪ‪ ،‬ﻭﻁﺒﻘﻪ ﺍﻟﺘﺎﺳﻴﺲ(‪.‬‬
‫‪ -١‬ﺍﺧﺘﺒﺎﺭ ﺍﻟﺒﺮﻭﻛﺘﻮﺭ ﺍﻟﻘﻴﺎﺳﻲ‪  .‬‬
‫‪ -٢‬ﺍﺧﺘﺒﺎﺭ ﺍﻟﺒﺮﻭﻛﺘﻮﺭ ﺍﻟﻤﻌﺪﻝ‪.‬‬
‫‪ -٣‬ﺍﺧﺗﺑﺎﺭ ﻧﺳﺑﻪ ﺗﺣﻣﻳﻝ ﻛﺎﻟﻳﻔﻭﺭﻧﻳﺎ‪  .‬‬
‫ﺧﺎﻣﺴﺎ‪ :‬ﺍﻟﺘﺠﺎﺭﺏ ﺍﻟﻤﻌﻤﻠﻴﺔ ﻟﻠﺨﻠﻄﺎﺕ ﺍﻻﺳﻔﻠﺘﻴﻪ‪.‬‬
‫‪ -١‬ﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ ﺍﻟﻛﻠﻲ ﻟﻠﻘﻭﺍﻟﺏ ﺍﻻﺳﻔﻠﺗﻳﻪ‪  .‬‬
‫‪ -٢‬ﺗﺣﺿﻳﺭ ﻗﻭﺍﻟﺏ ﻣﺎﺭﺷﺎﻝ‪  .‬‬
‫‪ -٣‬ﺍﺧﺗﺑﺎﺭ ﻣﺎﺭﺷﺎﻝ ﻟﻠﻘﻭﺍﻟﺏ ﺍﻻﺳﻔﻠﺗﻳﻪ‪  .‬‬

‫ﺳﺎﺩﺳﺎ‪ :‬ﺍﻟﺘﺠﺎﺭﺏ ﺍﻟﺤﻘﻠﻴﺔ ﻟﻠﻄﺒﻘﺎﺕ ﺍﻟﻤﻔﻜﻜﻪ )ﺍﻻﺳﺎﺱ‪ ،‬ﺍﻻﺳﺎﺱ ﺍﻟﻤﺴﺎﻋﺪ‪ ،‬ﻭﻁﺒﻘﻪ ﺍﻟﺘﺎﺳﻴﺲ(‪.‬‬
‫‪ -١‬ﺍﺧﺗﺑﺎﺭ ﺍﻟﻣﺧﺭﻭﻁ ﺍﻟﺭﻣﻠﻲ‪  .‬‬
‫‪ -٢‬ﺍﺧﺗﺑﺎﺭ ﻟﻭﺡ ﺍﻟﺗﺣﻣﻳﻝ‪  .‬‬

‫ﺳﺎﺑﻌﺎ‪ :‬ﺍﻟﺘﻘﺮﻳﺮ‪.‬‬
‫ﺍﻟﺗﺟﺎﺭﺏ ﻣﺭﻓﻘﻪ ﺑﻧﻣﻭﺫﺝ ﻟﺗﺳﺟﻳﻝ ﻧﺗﺎﺋﺞ ﺍﻻﺧﺗﺑﺎﺭ‬

‫‪ ‬‬

‫‪ ‬‬
 

‫ﺑﻳﺎﻧﺎﺕ ﺍﺟﻬﺯﻩ ﺍﻟﻣﻌﻣﻝ‬ 


 

Producing 
ID  Equipment  Model  Serial No. 
Company  
1  Centrifuge Extractor  ‐  ‐  ‐ 
2  Los Angeles Test  Control  D‐500  86040671 
3  Proctor Mechanical Hammer  Soil Test  CN‐4235‐8  8952 
1088 Or 
4  California Bearing Ratio  Soil Test  CI‐4724 
1988 
5  Saybolt_Furol Viscometer  Control  81‐80121  08008574 
6  Marshall  Control  B29‐B31  ‐ 
7  Marshall  ELE  27‐1559  35187 
8  California Bearing Ratio  Control  76‐Q08021c  09004366 
9  Cutter  Tnakita  ‐  87‐0000170 
10  Mechanical Shaker  Control  D403  88040625 
11  Marshall Mechanical Hammer  Control  B42  90040874 
12  Rotational Viscometer  ELE  RVDV‐IIIU  8496631 
13  Penetration  Control  B101/A  88010124 
 
‫ﺗﺟﺭﺑﻪ ﺭﻗﻡ‪‐١‐ ‬‬
‫ﺍﻟﺗﺣﻠﻳﻝ ﺍﻟﻣﻧﺧﻠﻲ ﻟﻠﺭﻛﺎﻡ‬
‫‪  Sieve Analysis of Aggregates‬‬
‫‪ASTM C136‬‬
‫‪ ‬ﺍﻟﻐﺭﺽ ‪ ‬‬
‫ﻟﺗﺣﺩﻳﺩ ﻣﻘﺎﺱ ﺣﺑﻳﺑﺎﺕ ﺍﻟﺭﻛﺎﻡ ﺍﻟﻧﺎﻋﻡ ﻭﺍﻟﺧﺷﻥ ﺑﻭﺍﺳﻁﻪ ﺍﻟﻧﺧﻝ ﺍﻟﺟﺎﻑ‪.‬‬
‫‪ ‬ﺍﻻﻫﻣﻳﺔ ﻭﺍﻻﺳﺗﺧﺩﺍﻡ ‪ ‬‬
‫ﻳﺳﺗﺧﺩﻡ ﻫﺫﺍ ﺍﻻﺧﺗﺑﺎﺭ ﻟﺗﺣﺩﻳﺩ ﺗﺩﺭﺝ ﺍﻟﻣﻭﺍﺩ ﺍﻟﻣﺳﺗﺧﺩﻣﺔ ﻣﺛﻝ ﺍﻟﺭﻛﺎﻡ‪ .‬ﻟﻠﺗﺄﻛﺩ ﺍﻥ ﻣﻘﺎﺱ ﺍﻟﺭﻛﺎﻡ ﻣﻁﺎﺑﻖ ﻟﻠﻣﺗﻁﻠﺑﺎﺕ‪.‬‬ ‫‪‬‬
‫‪ ‬ﺍﻻﺟﻬﺯﺓ ‪ ‬‬
‫ﻣﻳﺯﺍﻥ‪ .‬ﻻ ﺗﻘﻝ ﺩﻗﺗﻪ ﻋﻥ ‪ ٠٬٥‬ﺟﻡ ﻟﻠﺭﻛﺎﻡ ﺍﻟﺧﺷﻥ‪ ٠٬١ ،‬ﺟﻡ ﻟﻠﺭﻛﺎﻡ ﺍﻟﻧﺎﻋﻡ‪.‬‬ ‫‪‬‬
‫ﻣﻧﺎﺧﻝ‪  .‬‬ ‫‪‬‬
‫ﻫﺯﺍﺯ ﻣﻳﻛﺎﻧﻳﻛﻲ ﺷﻛﻝ )‪  .(١-١‬‬ ‫‪‬‬
‫ﻓﺭﻥ‪ .‬ﻗﺎﺩﺭ ﻟﻠﺣﻔﺎﻅ ﻋﻠﻲ ﺩﺭﺟﻪ ﺍﻟﺣﺭﺍﺭﺓ ﻣﻧﺗﻅﻣﺔ ‪ 110 5‬ﺩﺭﺟﻪ ﻣﺋﻭﻳﺔ‪  .‬‬ ‫‪‬‬
‫ﻣﻘﺳﻡ ﺍﻟﻌﻳﻧﺔ )‪ (Sample Splitter‬ﻟﺗﻘﻠﻳﻝ ﻛﻣﻳﻪ ﺍﻟﻣﻭﺍﺩ ﻟﻠﺣﺟﻡ ﺍﻟﻣﻁﻠﻭﺏ ﻟﺗﺣﻠﻳﻝ ﺍﻟﻣﻧﺧﻠﻲ ﺷﻛﻝ )‪-١‬‬ ‫‪‬‬
‫‪  .(٢‬‬

‫ﺻﻭﺭﻩ )‪ (١-١‬ﺍﻟﻬﺯﺍﺯ ﺍﻟﻣﻛﺎﻧﻳﻛﻲ‬ ‫ﺻﻭﺭﻩ )‪ (٢-١‬ﻁﺭﻳﻘﻪ ﺗﻘﺳﻳﻡ ﺍﻟﻌﻳﻧﺎﺕ‬


‫‪ ‬ﺗﺟﻬﻳﺯ ﺍﻟﻌﻳﻧﺔ ‪ ‬‬
‫ﺧﻠﻁ ﺍﻟﻌﻳﻧﺔ ﺟﻳﺩﺍ ﻭﺗﻘﻠﻳﻠﻬﺎ ﻟﻠﻛﻣﻳﺔ ﺍﻟﻣﻧﺎﺳﺑﺔ ﻟﻼﺧﺗﺑﺎﺭ‪ ،‬ﺑﺎﺳﺗﺧﺩﺍﻡ ﻣﻘﺳﻡ ﺍﻟﻌﻳﻧﺔ )‪ (Sample Splitter‬ﺍﻭ ﺗﻘﺳﻳﻡ ﺍﻻﺭﺑﻊ‬
‫)‪ .(quartering‬ﺍﻗﻝ ﻭﺯﻥ ﻟﻠﻌﻳﻧﻪ ﻛﻣﺎ ﻳﻠﻲ ‪،.....‬‬
‫ﺍﻗﻝ ﻭﺯﻥ )ﻛﺟﻡ(‬
‫‪٠٬١‬‬ ‫ﺍﻟﺭﻛﺎﻡ ﺍﻟﻧﺎﻋﻡ )ﻋﻠﻲ ﺍﻻﻗﻝ ‪ %٩٥‬ﻣﺎﺭ ﻣﻥ ﺍﻟﻣﻧﺧﻝ ‪ ٢٬٣٦‬ﻣﻡ )‪((٨ #‬‬
‫‪٠٬٥‬‬ ‫ﺍﻟﺭﻛﺎﻡ ﺍﻟﻧﺎﻋﻡ )ﻋﻠﻲ ﺍﻻﻗﻝ ‪ %٨٥‬ﻣﺭ ﻣﻥ ﺍﻟﻣﻧﺧﻝ ‪ ٤٬٧٥‬ﻣﻡ )‪((٤ #‬‬
‫‪١‬‬ ‫‪٣‬‬
‫ﺍﻟﺭﻛﺎﻡ ﺍﻟﺧﺷﻥ )ﺍﻟﻣﻘﺎﺱ ﺍﻻﻋﺗﺑﺎﺭﻱ ﺍﻻﻛﺑﺭ ‪ ٩٫٥‬ﻣﻡ )‪ #‬ﺑﻭﺻﻪ((‬
‫‪٢‬‬ ‫ﺍﻟﺭﻛﺎﻡ ﺍﻟﺧﺷﻥ )ﺍﻟﻣﻘﺎﺱ ﺍﻻﻋﺗﺑﺎﺭﻱ ﺍﻻﻛﺑﺭ ‪ ١٢٬٥‬ﻣﻡ )‪ #‬ﺑﻭﺻﻪ((‬
‫‪٥‬‬ ‫‪٣‬‬
‫ﺍﻟﺭﻛﺎﻡ ﺍﻟﺧﺷﻥ )ﺍﻟﻣﻘﺎﺱ ﺍﻻﻋﺗﺑﺎﺭﻱ ﺍﻻﻛﺑﺭ ‪ ١٩‬ﻣﻡ )‪ #‬ﺑﻭﺻﻪ((‬
‫‪١٠‬‬ ‫ﺍﻟﺭﻛﺎﻡ ﺍﻟﺧﺷﻥ )ﺍﻟﻣﻘﺎﺱ ﺍﻻﻋﺗﺑﺎﺭﻱ ﺍﻻﻛﺑﺭ ‪ ٢٥‬ﻣﻡ )‪ ١ #‬ﺑﻭﺻﻪ((‬
‫‪١٥‬‬ ‫ﺍﻟﺭﻛﺎﻡ ﺍﻟﺧﺷﻥ )ﺍﻟﻣﻘﺎﺱ ﺍﻻﻋﺗﺑﺎﺭﻱ ﺍﻻﻛﺑﺭ ‪ ٣٧٬٥‬ﻣﻡ )‪((١ #‬‬
‫‪ ‬ﺧﻁﻭﺍﺕ ﺍﻻﺧﺗﺑﺎﺭ ‪ ‬‬
‫‪ .١‬ﺗﺟﻔﻳﻑ ﻋﻳﻧﺔ ﺍﻟﺭﻛﺎﻡ ﺣﺗﻲ ﻳﺛﺑﺕ ﻭﺯﻧﻬﺎ ﻋﻧﺩ ﺩﺭﺟﻪ ﺣﺭﺍﺭﻩ ‪ 110 5‬ﺩﺭﺟﻪ ﻣﺋﻭﻳﺔ‪ ،‬ﺛﻡ ﺗﺑﺭﺩ ﻟﺩﺭﺟﻪ ﺣﺭﺍﺭﻩ ﺍﻟﻐﺭﻓﺔ‪  .‬‬
‫‪ .٢‬ﺗﺟﻬﻳﺯ ﺍﻟﻣﻧﺎﺧﻝ ﻹﺟﺭﺍء ﺍﻻﺧﺗﺑﺎﺭ ﺍﻟﺗﻲ ﺗﺗﺭﺍﻭﺡ ﻣﻘﺎﺳ ﺗﻬﺎ ﺑ ﺎﻟﻣﻳﻠﻳﻣﺗﺭ ‪،١٬١٨ ،٢٬٣٦ ،٤٬٧٥ ،٩٬٥ ،١٢٬٥ ،١٩ ،٢٥ ،٣٧٬٥‬‬
‫‪1‬‬ ‫‪3‬‬ ‫‪1‬‬ ‫‪3‬‬
‫‪ ،٠٬١٥ ،٠٬٣ ،٠٬٦‬ﻭ‪ ٠٬٠٧٥‬ﻣ ﻡ ) ﺑﻭﺻﻪ‪ ،‬ﺑﻭﺻﻪ‪ ،‬ﺑﻭﺻﻪ‪١،‬ﺑﻭﺻﻪ‪ ،‬ﺑﻭﺻﻪ‪# ٥٠ # ،٣٠ # ،١٦ # ،٨ # ،٤ # ١،‬‬
‫‪2‬‬ ‫‪4‬‬ ‫‪2‬‬ ‫‪8‬‬
‫‪ ١٠٠‬ﻭ ‪  .(٢٠٠ #‬‬
‫‪ .٣‬ﺗﺭﺗﻳﺏ ﺍﻟﻣﻧﺎﺧﻝ ﺗﻧﺎﺯﻟﻳﺎ )ﺣﺳﺏ ﻣﻘﺎﺱ ﺍﻟﻣﻧﺧﻝ(‪ ،‬ﻭﻭﺿﻊ ﻋﻳﻧﺔ ﺍﻟﺭﻛﺎﻡ ﻋﻠﻲ ﺍﻟﻣﻧﺧﻝ‪  .‬‬
‫‪ .٤‬ﻫﺯ ﺍﻟﻣﻧﺎﺧﻝ ﻳﺩﻭﻳﺎ ﺍﻭ ﻣﻳﻛﺎﻧﻳﻛﻳﺎ ﻟﻔﺗﺭﻩ ﻣﻧﺎﺳﺑﻪ )ﺣﺗﻲ ﻳﻘﻝ ﻣﺭﻭﺭ ﺣﺑﻳﺑﺎﺕ ﺍﻟﺭﻛﺎﻡ ﻋﻥ ‪%١‬‬
‫ﻣﻥ ﺍﻟﻌﻳﻧﺔ ﺍﻟﻣﺣﺟﻭﺯﺓ ﻋﻠﻲ ﺍﻟﻣﻧﺧﻝ ﺧﻼﻝ ‪ ١‬ﺩﻗﻳﻘﺔ(‪  .‬‬
‫‪ .٥‬ﺣﺳﺎﺏ ﻭﺯﻥ ﺍﻟﻣﺣﺟﻭﺯ ﻋﻠﻲ ﻛﻝ ﻣﻧﺧﻝ ﺷﻛﻝ )‪  .(٣-١‬‬
‫‪ .٦‬ﻳﺗﻡ ﺣﺳﺎﺏ ﻣﺟﻣﻭﻉ ﺍﻭﺯﺍﻥ ﺍﻟﻣﻭﺍﺩ ﺍﻟﻣﺣﺟﻭﺯﺓ ﻋﻠﻲ ﺍﻟﻣﻧﺎﺧﻝ ﺑﻌﺩ ﺍﻟﻧﺧ ﻝ ﻭﻣﻘﺎﺭﻧﺗﻬ ﺎ ﺑ ﻭﺯﻥ‬
‫ﺍﻟﻌﻳﻧﺔ ﻗﺑﻝ ﺍﻻﺧﺗﺑ ﺎﺭ ﺇﺫﺍ ﻛ ﺎﻥ ﺍﻻﺧ ﺗﻼﻑ ﺍﻛﺑ ﺭ ﻣ ﻥ ‪ %٠٬٣‬ﻣ ﻥ ﻭﺯﻥ ﺍﻟﻌﻳﻧ ﺔ ﺍﻻﺻ ﻠﻲ ﻻ‬
‫ﻳﻌﺩ ﺑﻧﺗﺎﺋﺞ ﺍﻟﺗﺟﺭﺑﺔ‪  .‬‬
‫𝑊‬ ‫𝑊‬
‫𝑠𝑒𝑠𝑠𝑜𝐿 ‪%‬‬ ‫‪𝑥100 0.3% ‬‬
‫𝑊‬
‫ﺣﻳﺙ ‪:‬‬

‫ﻧﺳﺑﻪ ﺍﻟﻔﺎﻗﺩ ﻓﻲ ﺍﻟﻌﻳﻧﺔ ﺍﺛﻧﺎء ﺍﻻﺧﺗﺑﺎﺭ‪.‬‬ ‫‪: %Losses‬‬


‫ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ ﺍﻟﺟﺎﻑ ﻗﺑﻝ ﺍﻻﺧﺗﺑﺎﺭ‪.‬‬ ‫‪: Wbefore‬‬
‫ﺻﻭﺭﻩ )‪ (٣-١‬ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ‬ ‫ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ ﺑﻌﺩ ﺍﻻﺧﺗﺑﺎﺭ‪.‬‬ ‫‪: Wafter‬‬
‫ﺍﻟﻣﺣﺟﻭﺯﺓ ﻋﻠﻲ ﺍﻟﻣﻧﺎﺧﻝ‬
‫‪ .٧‬ﺣﺳﺎﺏ ﻧﺳﺑﺔ ﺍﻟﻣﺣﺟﻭﺯ )‪ (%‬ﻋﻠﻲ ﻛﻝ ﻣﻧﺧﻝ ﺑﻠﻠﻧﺳﺑﺔ ﻟﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ ﺍﻟﻛﻠﻲ‪.‬‬
‫ﻭﺯﻥ ﺍﻟﻣﺣﺟﻭﺯ‬
‫‪%‬‬ ‫‪𝑥100‬‬
‫ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ‬
‫‪ ‬ﺍﻟﻧﺗﺎﺋﺞ ‪:‬‬
‫‪ .١‬ﺣﺳﺎﺏ ﻧﺳﺑﺔ ﺍﻟﻣﺎﺭ‪ ،‬ﻧﺳﺑﻪ ﺍﻟﻣﺣﺟﻭﺯ ﺍﻟﻛﻠﻲ ﺍﻭ ﻧﺳﺑﻪ ﺍﻟﻣﻘﺎﺳﺎﺕ ﺍﻟﻣﺧﺗﻠﻔﺔ ﻷﻗﺭﺏ ‪ % ٠٬١‬ﺑﺎﻟﻧﺳﺑﺔ ﻟﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ ﺍﻻﺻﻠﻲ‪  .‬‬
‫‪ .٢‬ﺭﺳﻡ ﺍﻟﻌﻼﻗﺔ ﺑﻳﻥ ﻣﻘﺎﺱ ﺍﻟﻣﻧﺧﻝ ﻭﻧﺳﺑﻪ ﺍﻟﻣﺎﺭ ﻋﻠﻲ ﻣﻧﺣﻧﻲ )‪  .(Semi‐log scale‬‬
‫‪ .٣‬ﺭﺳﻡ ﺍﻟﻌﻼﻗﺔ ﺑﻳﻥ ﻣﻘﺎﺱ ﺍﻟﻣﻧﺧﻝ ﻭﻧﺳﺑﻪ ﺍﻟﻣﺎﺭ ﻋﻠﻲ ﻣﻧﺣﻧﻲ )‪  .(0.45 Power gradation‬‬
‫‪ .٤‬ﺣﺳﺎﺏ ﻣﻌﺎﻣﻝ ﺍﻟﻧﻌﻭﻣﺔ‪  .‬‬
‫‪ ‬ﺍﻟﺗﻘﺭﻳﺭ ‪ ‬‬
‫‪ .١‬ﻧﺳﺑﻪ ﺍﻟﻣﻭﺍﺩ ﺍﻟﻣﺣﺟﻭﺯﺓ ﻋﻠﻲ ﺍﻟﻣﻧﺎﺧﻝ‪ ،‬ﺍﻟﻧﺳ ﺑﺔ ﺍﻟﺗﺟﻣﻳﻌﻳ ﺔ ﻟﻠﻣﺣﺟ ﻭﺯ ﻋﻠ ﻲ ﻛ ﻝ ﻣﻧﺧ ﻝ ﺍﻭ ﻧﺳ ﺑﻪ ﺍﻟﻣ ﺎﺭ ﻣ ﻥ ﻛ ﻝ ﻣﻧﺧ ﻝ‪ .‬ﻳ ﺗﻡ‬
‫ﺗﻘﺭﻳﺏ ﻧﺳﺏ ﺍﻟﻣﻭﺍﺩ ﻷﻗﺭﺏ ﺭﻗﻡ ﺻﺣﻳﺢ‪ ،‬ﺍﻻ ﺍﺫﺍ ﻛﺎﻥ ﻧﺳﺑﻪ ﺍﻟﻣ ﺎﺭ ﻣ ﻥ ﺍﻟﻣﻧﺧ ﻝ ‪ ٠٬٠٧٥‬ﻣ ﻡ )ﺭﻗ ﻡ ‪ (٢٠٠‬ﺍﻗ ﻝ ﻣ ﻥ ‪%١٠‬‬
‫ﻳﺗﻡ ﺍﻟﺗﻘﺭﻳﺏ ﺍﻟﻧﺳﺏ ﻷﻗﺭﺏ ‪  .% ٠٬١‬‬
‫‪ .٢‬ﺭﺳﻡ ﺍﻟﻌﻼﻗﺔ ﺑﻳﻥ ﻣﻘﺎﺱ ﺍﻟﻣﻧﺧﻝ ﻭﻧﺳﺑﺔ ﺍﻟﻣﺎﺭ ﻋﻠﻲ ﻣﻧﺣﻧﻲ )‪ (Semi‐log‬ﻭ )‪  .(0.45 power gradation‬‬
‫‪ .٣‬ﺣﺳﺎﺏ ﻣﻌﺎﻣﻝ ﺍﻟﻧﻌﻭﻣﺔ ﻷﻗﺭﺏ ‪  .٠٬٠١‬‬
‫‪Sieve Analysis Test ‬‬

‫ﻧﺳﺑﺔ ﺍﻟﻣﺣﺟﻭﺯ‬ ‫ﻧﺳﺑﺔ‬ ‫ﻭﺯﻥ‬


‫ﻧﺳﺑﺔ ﺍﻟﻣﺎﺭ ﺍﻟﻛﻠﻲ‬ ‫ﻗﻁﺭ ﺍﻟﻣﻧﺧﻝ‬ ‫ﺭﻗﻡ ﺍﻟﻣﻧﺧﻝ‬
‫ﺍﻟﻛﻠﻲ‬ ‫ﺍﻟﻣﺣﺟﻭﺯ ‪ ‬‬ ‫ﺍﻟﻣﺣﺟﻭﺯ‬
‫‪ ‬‬ ‫‪٣٧٬٥‬‬ ‫‪ 1 2‬ﺑﻭﺻﻪ‪١‬‬

‫‪٢٥‬‬ ‫ﺑﻭﺻﻪ‪١‬‬

‫‪١٩‬‬ ‫‪ 3 4‬ﺑﻭﺻﻪ‬

‫‪١٢٬٥‬‬ ‫‪ 1 2‬ﺑﻭﺻﻪ‬

‫‪٩٬٥‬‬ ‫‪ 3 8‬ﺑﻭﺻﻪ‬

‫‪٤٬٧٥‬‬ ‫‪٤#‬‬

‫‪٢٬٣٦‬‬ ‫‪٨#‬‬

‫‪١٬١٨‬‬ ‫‪١٦ #‬‬

‫‪٠٬٦‬‬ ‫‪٣٠ #‬‬

‫‪٠٬٣‬‬ ‫‪٥٠ #‬‬

‫‪٠٬١٥‬‬ ‫‪١٠٠ #‬‬

‫‪٠٬٠٧٥‬‬ ‫‪٢٠٠ #‬‬

‫ﺍﻟﻣﺟﻣﻭﻉ‬
‫ﺻﻭﺭﻩ )‪Semi‐log gradation chart (٤-١‬‬
‫ﺍﻟﻣﻘﺎﺱ‬ ‫ﻧﺳﺑﺔ‬
‫‪Pi = ‬‬ ‫ﻧﺳﺑﺔﺍﻟﻣﺣﺟﻭﺯ ﻧﺳﺑﺔﺍﻟﻣﺣﺟﻭﺯﺍﻟﻛﻠﻲ‬ ‫ﻭﺯﻧﺎﻟﻣﺣﺟﻭﺯ‬
‫‪ ‬‬
‫‪D0.45‬‬ ‫ﺍﻻﻋﺗﺑﺎﺭﻱ ﺍﻻﻛﺑﺭ‬ ‫ﺍﻟﻣﺎﺭ‬ ‫‪ %‬‬ ‫‪ %‬‬ ‫)ﺟﻡ( ‪ ‬‬
‫ﺭﻗﻣﺎﻟﻣﻧﺧﻝ ‪  ‬ﻗﻁﺭﺍﻟﻣﻧﺧﻝ‬
‫‪100(di/D)0.45‬‬
‫)ﻣﻡ(‬ ‫ﺍﻟﻛﻠﻲ ‪%‬‬
‫‪ ‬‬ ‫‪5.10874‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪  37,5‬‬ ‫‪ ‬ﺑﻭﺻﻪ ‪١⁄٢١‬‬
‫‪ ‬‬ ‫‪  4.2567‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪  25‬‬ ‫ﺑﻭﺻﻪ ‪  ١‬‬
‫‪ ‬‬ ‫‪3.76218‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪  19‬‬ ‫ﺑﻭﺻﻪ ‪  ٣⁄٤‬‬
‫‪ ‬‬ ‫‪3.11609‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪  12,5‬‬ ‫ﺑﻭﺻﻪ ‪  ١⁄٢‬‬
‫‪ ‬‬ ‫‪2.75407‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪  9,5‬‬ ‫ﺑﻭﺻﻪ ‪  ٣⁄٨‬‬
‫‪ ‬‬ ‫‪  2.0161‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪  4,75‬‬ ‫‪  # 4‬‬
‫‪ ‬‬
‫‪ ‬‬ ‫‪1.47167‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪  2,36‬‬ ‫‪  # 8‬‬
‫‪ ‬‬ ‫‪1.07733‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪  1,18‬‬ ‫‪  # 16‬‬
‫‪ ‬‬ ‫‪0.79464‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪  0,6‬‬ ‫‪  # 30‬‬
‫‪ ‬‬ ‫‪0.58171‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪  0,3‬‬ ‫‪  # 50‬‬
‫‪ ‬‬ ‫‪0.42583‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪  ٠٬١٥‬‬ ‫‪  # 100‬‬
‫‪ ‬‬ ‫‪0.31173‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪  ٠٬٠٧٥‬‬ ‫‪  # 200‬‬
‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫‪ ‬‬ ‫ﺍﻟﻣﺟﻣﻭﻉ‬
‫‪ ‬‬

‫ﺷﻛﻝ )‪0.45 power gradation Chart (٥-١‬‬


‫ﺗﺟﺭﺑﺔ ﺭﻗﻡ ‪-٢-‬‬
‫ﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ ﻭﺍﻻﻣﺗﺻﺎﺹ ﻟﻠﺭﻛﺎﻡ ﺍﻟﺧﺷﻥ‬
‫‪  Specific Gravity and Absorption of Coarse Aggregate‬‬
‫‪ASTM C127‬‬
‫‪ ‬ﺍﻟﻐﺭﺽ ‪:‬‬
‫ﻟﺣﺳﺎﺏ ﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ ﺍﻟﻛﻠ ﻲ )‪ (Bulk Specific Gravity‬ﻟﻠﺭﻛ ﺎﻡ ﺍﻟﺧﺷ ﻥ‪ ،‬ﻭﻧﺳ ﺑﻪ ﺍﻣﺗﺻﺎﺻ ﻪ ﻟﻠﻣﻳ ﺎﻩ )‪(Water Absorption‬‬
‫ﻭﺍﻟﺗﻲ ﺗﺗﻣﺛﻝ ﻓﻲ ﺍﻟﻛﺛﺎﻓﺔ ﺍﻟﻧﻭﻋﻳﺔ‪ ،‬ﻭﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ ﺍﻟﻅﺎﻫﺭﻱ )‪(Apparent Specific Gravity‬ﻭ ﺍﻟ ﻭﺯﻥ ﺍﻟﻧ ﻭﻋﻲ )ﻣﺷ ﺑﻌﺔ ﺟﺎﻓ ﻪ‬
‫ﺍﻟﺳﻁﺢ( )‪.(S.S.D. Specific Gravity‬‬
‫ﺍﻷﻫﻣﻳﺔ ﻭﺍﻻﺳﺗﺧﺩﺍﻡ ‪:‬‬ ‫‪‬‬
‫ﻳﺳﺗﺧﺩﻡ ﺍﻟ ﻭﺯﻥ ﺍﻟﻧ ﻭﻋﻲ ﻓ ﻲ ﺗﺣﺩﻳ ﺩ ﺍﻟﺣﺟ ﻡ ﺍﻟﻣﺷ ﻐﻭﻝ ﺑﻭﺍﺳ ﻁﻪ ﺍﻟﺭﻛ ﺎﻡ ﻓ ﻲ ﺍﻟﺧﻠﻁ ﺎﺕ ﺍﻟﻣﺧﺗﻠﻔ ﺔ ﺍﻟﺗ ﻲ ﺗﺗﻛ ﻭﻥ ﻣ ﻥ ﺍﻟﺭﻛ ﺎﻡ‪ ،‬ﺗﺷ ﻣﻝ‬ ‫‪‬‬
‫ﺍﻟﺧﺭﺳﺎﻧﺔ ﺍﻻﺳﻣﻧﺗﻳﺔ‪ ،‬ﺍﻟﺧﺭﺳﺎﻧﺔ ﺍﻻﺳﻔﻠﺗﻳﻪ ﻭﺍﻱ ﻣﺧﻠﻭﻁ ﻳﺗﻡ ﺗﺣﻠﻳﻠﻪ ﻋﻠﻲ ﺍﺳﺎﺱ ﺍﻟﺣﺟﻡ ﺍﻟﻣﻁﻠﻖ‪.‬‬
‫ﺍﻟﻛﺛﺎﻓﺔ ﺍﻟﻧﻭﻋﻳﺔ )ﻣﺷﺑﻌﺔ ﻭﺍﻟﺳﻁﺢ ﺟﺎﻑ( ﺗﺳﺗﺧﺩﻡ ﺍﺫﺍ ﻛﺎﻧﺕ ﺍﻟﻌﻳﻧﺔ ﺭﻁﺑﻪ‪.‬‬ ‫‪‬‬
‫ﻭﻧﺳﺑﻪ ﺍﻻﻣﺗﺻﺎﺹ ﺗﺳ ﺗﺧﺩﻡ ﻟﺣﺳ ﺎﺏ ﺍﻟﺗﻐﻳ ﺭ ﻓ ﻲ ﻭﺯﻥ ﺍﻟﺭﻛ ﺎﻡ ﻧﺗﻳﺟ ﺔ ﺍﻣﺗﺻ ﺎﺹ ﺍﻟﻣﻳ ﺎﻩ ﻓ ﻲ ﺍﻟﻔﺭﺍﻏ ﺎﺕ ﺍﻟﻣﺳ ﺎﻣﻳﺔ ﻓ ﻲ ﺍﻟﺟﺯﻳﺋ ﺎﺕ‬ ‫‪‬‬
‫ﺍﻟﻣﻛﻭﻧﺔ ﻣﻘﺎﺭﻧﺔ ﺑﺎﻟﺣﺎﻟﺔ ﺍﻟﺟﺎﻓﻪ‪  .‬‬
‫‪ ‬ﻣﻳﺯﺍﻥ‬
‫ﺍﻻﺟﻬﺯﺓ ﺍﻟﻣﺳﺗﺧﺩﻣﺔ ‪:‬‬ ‫‪‬‬
‫ﻣﻳﺯﺍﻥ ﺩﻗﺗﻪ ‪ % ٠٬٠٥‬ﻣﻥ ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ ﺍﻭ ‪ ٠٬٥‬ﺟﻡ ﺍﻳﻬﻣﺎ ﺍﻛﺑﺭ‪.‬‬ ‫‪‬‬
‫‪ ‬ﺳﻠﺔ‬
‫ﺳﻠﻪ)‪ ٣٬٣٥‬ﻣﻡ )‪.((٦ #‬‬ ‫‪‬‬
‫ﺧﺯﺍﻥ ﻣﻳﺎﻩ‪.‬‬ ‫‪‬‬
‫ﺧﺯﺍﻥ‬ ‫ﻣﻧﺧﻝ )‪ ٤٬٧٥‬ﻣﻡ( ﺭﻗﻡ ‪ ٤‬ﺍﻭ ﺍﻱ ﻣﻘﺎﺱ ﻣﻁﻠﻭﺏ‪  .‬‬ ‫‪‬‬
‫‪ ‬ﺍﻟﻣﻳﺎﻩ‬ ‫‪ ‬ﺗﺟﻬﻳﺯ ﺍﻟﻌﻳﻧﺔ ‪:‬‬
‫‪ .١‬ﺧﻠﻁ ﺍﻟﻌﻳﻧ ﺔ ﺟﻳ ﺩﺍ ﻭﺗﻘﻠﻳﻠﻬ ﺎ ﺍﻟ ﻲ ﺍﻟﻛﻣﻳ ﺔ ﺍﻟﻣﻁﻠﻭﺑ ﺔ ﺗﻘﺭﻳﺑ ﺎ ﺑﺎﺳ ﺗﺧﺩﺍﻡ ﻣﻘﺳ ﻡ ﺍﻟﻌﻳﻧ ﺔ ) ‪Sample ‬‬
‫‪ (Splitter‬ﺍﻭ ﻁﺭﻳﻘﺔ ﺍﻻﺭﺑﻊ )‪.(Quartering‬‬
‫‪ .٢‬ﺭﻓ ﺽ ﺍﻟﻣ ﻭﺍﺩ ﺍﻟﻣ ﺎﺭﺓ ﻣ ﻥ ﺍﻟﻣﻧﺧ ﻝ ‪ ٤٬٧٥‬ﻣ ﻡ )ﺭﻗ ﻡ ‪ (٤‬ﻭﻏﺳ ﻝ ﺍﻟﻌﻳﻧ ﺔ ﺟﻳ ﺩﺍ ﻹﺯﺍﻟ ﻪ ﺍﻟﻐﺑ ﺎﺭ‬

‫ﺷﻛﻝ )‪ (١-٢‬ﺍﻟﻣﻳﺯﺍﻥ ﻭ ﺍﻟﺳﻠﺔ‬ ‫ﻭﺍﻟﻣﻭﺍﺩ ﺍﻟﻌﺎﻟﻘﺔ ﻋﻠﻲ ﺳﻁﺢ ﺍﻟﺭﻛﺎﻡ‪.‬‬


‫ﺎﺭﻱ‬ ‫ﺍﻻﻋﺗﺑ‬ ‫ﻭﺧﺯﺍﻥ ﺍﻟﻣﻳﺎﻩ ﺍﻟﻣﺳﺗﺧﺩﻡ ﻓﻲ ﺣﺳﺎﺏ‬
‫‪ .٣‬ﺍﻗ ﻝ ﻭﺯﻥ ﻟﻌﻳﻧ ﺔ ﺍﻻﺧﺗﺑ ﺎﺭ ﺍﻟﻣﺳ ﺗﺧﺩﻣﺔ ﺗﻌﺗﻣ ﺩ ﻋﻠ ﻲ ﺍﻟﻣﻘ ﺎﺱ‬
‫ﺍﻻﻛﺑﺭ )‪ (NAMS‬ﻛﻣﺎ ﻳﻠﻲ‪  ،....‬‬
‫ﺍﻟﻛﺛﺎﻓﺔ ﺍﻟﻧﻭﻋﻳﺔ ﻭﻧﺳﺑﺔ ﺍﻻﻣﺗﺻﺎﺹ ‪ ‬‬
‫ﺍﻗﻝ ﻭﺯﻥ ﻟﻠﻌﻳﻧﺔ‪ ،‬ﻛﺟﻡ‬ ‫ﺍﻟﻣﻘﺎﺱ ﺍﻻﻋﺗﺑﺎﺭﻱ ﺍﻻﻛﺑﺭ‪ ،‬ﻣﻡ‬
‫‪٢‬‬ ‫‪١٢٬٥‬‬
‫‪٣‬‬ ‫‪١٩٬٠‬‬
‫‪٤‬‬ ‫‪٢٥٬٠‬‬
‫‪٥‬‬ ‫‪٣٧٬٥‬‬ ‫‪ ‬‬
‫ﺧﻁﻭﺍﺕ ﺍﻻﺧﺗﺑﺎﺭ‬ ‫‪‬‬
‫ﻏﻣﺭ ﺍﻟﺭﻛﺎﻡ ﻓﻲ ﺍﻟﻣﻳﺎﻩ ﻋﻧﺩ ﺩﺭﺟﻪ ﺣﺭﺍﺭ ﺍﻟﻐﺭﻓﺔ ﻟﻣﺩﻩ ‪ 24 4‬ﺳﺎﻋﻪ‪.‬‬ ‫‪‬‬
‫ﺇﺯﺍﻟﻪ ﺍﻟﻌﻳﻧﺔ ﻣﻥ ﺍﻟﻣﻳﺎﻩ‪ ،‬ﻭﻓﺭﺩﻫﺎ ﻋﻠﻲ ﻗﻁﻌﻪ ﻣ ﻥ ﺍﻟﻘﻣ ﺎﺵ ﺍﻟﻣﺑﺗﻠ ﺔ ﺣﺗ ﻲ ﻳﺟ ﻑ ﺳ ﻁﺣﻬﺎ )ﻣﺷ ﺑﻌﺔ ﺟﺎﻓ ﻪ ﺍﻟﺳ ﻁﺢ(‪ .‬ﻣﺳ ﺢ ﺍﻟﺣﺑﻳﺑ ﺎﺕ‬ ‫‪‬‬
‫ﺍﻟﻛﺑﻳﺭﺓ‪.‬‬
‫ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ )ﻣﺷﺑﻌﺔ ﺟﻔﺔ ﺍﻟﺳﻁﺢ( ﻭﻟﻳﻛﻥ )‪ .(B‬ﻳﺗﻡ ﺗﻘﺭﻳﺏ ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ ﻷﻗﺭﺏ ‪ ٠٬٥‬ﺟﻡ ﺍﻭ ‪ %٠٬٠٥‬ﺍﻳﻬﻣﺎ ﺍﻛﺑﺭ‪.‬‬ ‫‪‬‬
‫‪ 23‬ﺩﺭﺟ ﺔ ﻣﺋﻭﻳ ﺔ‪ ،‬ﻭﻟ ﻳﻛﻥ )‪ .(C‬ﻳ ﺗﻡ ﻫ ﺯ‬ ‫‪ ‬ﻭﺿ ﻊ ﺍﻟﻌﻳﻧ ﺔ ﻓ ﻲ ﺍﻟﺳ ﻠﺔ ﻟﺣﺳ ﺎﺏ ﻭﺯﻥ ﺍﻟﻌﻳﻧ ﺔ ﻓ ﻲ ﺍﻟﻣﻳ ﺎﻩ ﻋﻧ ﺩ ﺩﺭﺟ ﻪ ﺣ ﺭﺍﺭﺓ ‪1٧‬‬
‫ﺍﻟﻭﻋﺎء ﺑﻊ ﻏﻣﺭﻩ ﻓﻲ ﺍﻟﻣﻳﺎﻩ ﻹﺯﺍﻟﻪ ﺍﻟﻔﻘﺎﻗﻳﻊ ﺍﻟﻬﻭﺍﺋﻳﺔ ﻗﺑﻝ ﺗﺳﺟﻳﻝ ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ‪  .‬‬
‫‪ 110‬ﺩﺭﺟﺔ ﻣﺋﻭﻳﺔ‪ ،‬ﻭﻭﺯﻧﻬﺎ ﻭﻟﻳﻛﻥ )‪.(A‬‬ ‫‪ ‬ﺗﺟﻔﻳﻑ ﺍﻟﻌﻳﻧﺔ ﺣﺗﻲ ﻳﺛﺑﺕ ﻭﺯﻧﻬﺎ ﻋﻧﺩ ﺩﺭﺟﻪ ﺣﺭﺍﺭﺓ ‪5‬‬
‫‪ ‬ﺍﻟﺗﺣﻠﻳﻝ ﻭﺍﻟﻧﺗﺎﺋﺞ ‪  :‬‬
‫‪ ‬‬ ‫‪ .١‬ﺍﻟﻛﺛﺎﻓﺔ ﺍﻟﻧﻭﻋﻳﺔ =‬
‫ﺣﻳﺙ ‪:‬‬
‫‪ :A‬ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ ﺍﻟﺟﺎﻓﺔ ﻓﻲ ﺍﻟﻬﻭﺍء‪ ،‬ﺟﻡ‪.‬‬
‫‪ :B‬ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ ﻣﺷﺑﻌﺔ ﺑﺎﻟﻣﻳﺎﻩ ﺟﺎﻓﺔ ﺍﻟﺳﻁﺢ‪ ،‬ﺟﻡ‪.‬‬
‫‪ :C‬ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ ﺍﻟﻣﺷﺑﻌﺔ ﻓﻲ ﺍﻟﻣﻳﺎﻩ‪ ،‬ﺟﻡ‪.‬‬
‫‪ .٢‬ﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ )ﻣﺷﺑﻌﺔ ﺟﺎﻓﺔ ﺍﻟﺳﻁﺢ( =‬
‫‪ .٣‬ﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ ﺍﻟﻅﺎﻫﺭﻳﺔ =‬
‫‪  .100 x‬‬ ‫‪ .٤‬ﻧﺳﺑﻪ ﺍﻻﻣﺗﺻﺎﺹ ‪= %‬‬

‫‪ ‬ﺍﻟﺗﻘﺭﻳﺭ‬
‫‪ ‬ﺍﻟﻛﺛﺎﻓﺔ ﺍﻟﻧﻭﻋﻳﺔ‪.‬‬
‫‪ ‬ﺍﻟﻛﺛﺎﻓﺔ ﺍﻟﻧﻭﻋﻳﺔ )ﻣﺷﺑﻌﺔ ﺟﺎﻓﻪ ﺍﻟﺳﻁﺢ(‪.‬‬
‫‪ ‬ﺍﻟﻛﺛﺎﻓﺔ ﺍﻟﻧﻭﻋﻳﺔ ﺍﻟﻅﺎﻫﺭﻳﺔ‪.‬‬
‫‪ ‬ﻧﺳﺑﻪ ﺍﻻﻣﺗﺻﺎﺹ‪.‬‬
Specific Gravity Test of Coarse Aggregate 
 

Weight in Air  A =    gm 


S.S.D Weight  B =    gm 
Weight in Water  C =    gm 

Specific Gravity Values:
Bulk Specific Gravity  =  A/(B‐C)   
  =    gm/cm3 
S.S.D Specific Gravity  =  B/(B‐C)   
  =    gm/cm3 
Apparent Specific Gravity  =  A/(A‐C)   
  =    gm/cm3 

Water Absorption % 
Water Absorption   =  (B‐A)/A   
  =    % 
 
 
 

 
‫ﺗﺟﺭﺑﺔ ﺭﻗﻡ ‪-٣-‬‬
‫ﺍﻟﻛﺛﺎﻓﺔ ﺍﻟﻧﻭﻋﻳﺔ ﻭﺍﻻﻣﺗﺻﺎﺹ ﻟﻠﺭﻛﺎﻡ ﺍﻟﻧﺎﻋﻡ‬
‫‪  Specific Gravity and Absorption of Fine Aggregate‬‬
‫‪  ASTM C128‬‬
‫‪ ‬ﺍﻟﻐﺭﺽ ‪:‬‬
‫ﻟﺣﺳ ﺎﺏ ﺍﻟ ﻭﺯﻥ ﺍﻟﻧ ﻭﻋﻲ ﺍﻟﻛﻠ ﻲ)‪ (Bulk Specific Gravity‬ﻟﻠﺭﻛ ﺎﻡ ﺍﻟﻧ ﺎﻋﻡ‪ ،‬ﻭﻧﺳ ﺑﻪ ﺍﻣﺗﺻﺎﺻ ﻪ ﻟﻠﻣﻳ ﺎﻩ )‪(Water Absorption‬‬
‫ﻭﺍﻟﺗﻲ ﺗﺗﻣﺛﻝ ﻓﻲ ﺍﻟﻛﺛﺎﻓﺔ ﺍﻟﻧﻭﻋﻳﺔ‪ ،‬ﻭﺍﻟﻛﺛﺎﻓﺔ ﺍﻟﻧﻭﻋﻳﺔ ﺍﻟﻅﺎﻫﺭﻳﺔ )‪ (Apparent Specific Gravity‬ﻭ ﺍﻟﻛﺛﺎﻓﺔ ﺍﻟﻧﻭﻋﻳﺔ )ﻣﺷﺑﻌﺔ ﺟﺎﻓﻪ‬
‫ﺍﻟﺳﻁﺢ( )‪.(S.S.D Specific Gravity‬‬
‫‪ ‬ﺍﻷﻫﻣﻳﺔ ﻭﺍﻻﺳﺗﺧﺩﺍﻡ ‪:‬‬
‫‪ ‬ﺗﺳﺗﺧﺩﻡ ﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ ﺍﻟﻛﻠﻲ ﻓﻲ ﺗﺣﺩﻳﺩ ﺍﻟﺣﺟﻡ ﺍﻟﻣﺷﻐﻭﻝ ﺑﻭﺍﺳﻁﻪ ﺍﻟﺭﻛﺎﻡ ﻓﻲ ﺍﻟﺧﻠﻁﺎﺕ ﺍﻟﻣﺧﺗﻠﻔﺔ ﺍﻟﺗﻲ ﺗﺗﻛﻭﻥ ﻣﻥ ﺍﻟﺭﻛﺎﻡ‪ ،‬ﺗﺷ ﻣﻝ‬
‫ﺍﻟﺧﺭﺳﺎﻧﺔ ﺍﻻﺳﻣﻧﺗﻳﺔ‪ ،‬ﺍﻟﺧﺭﺳﺎﻧﺔ ﺍﻻﺳﻔﻠﺗﻳﻪ ﻭﺍﻱ ﻣﺧﻠﻭﻁ ﻳﺗﻡ ﺗﺣﻠﻳﻠﻪ ﻋﻠﻲ ﺍﺳﺎﺱ ﺍﻟﺣﺟﻡ ﺍﻟﻣﻁﻠﻖ‪.‬‬
‫‪ ‬ﺍﻻﺟﻬﺯﺓ ﺍﻟﻣﺳﺗﺧﺩﻣﺔ ‪:‬‬
‫‪ ‬ﻣﻳﺯﺍﻥ ﺩﻗﺗﻪ ‪ % ٠٬٠٥‬ﻣﻥ ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ ﺍﻭ ‪ ٠٬٥‬ﺟﻡ ﺍﻳﻬﻣﺎ ﺍﻛﺑﺭ‪  .‬‬
‫‪ ‬ﺩﻭﺭﻕ )‪ (Pyconometer‬ﺳﻌﺗﻪ ‪ ٥٠٠‬ﺳﻡ‪  .٣‬‬
‫‪ ‬ﻗﺎﻟﺏ ﻣﺧﺭﻭﻁﻲ ﻧﺎﻗﺹ‪ .‬ﻗﻁﺭﻩ ﺍﻟﻌﻠﻭﻱ )‪ (٣ ± ٤٠‬ﻣﻡ ﻭﻗﺭﻩ ﺍﻟﺳﻔﻠﻲ )‪ (٣± ٩٠‬ﻣﻡ‪  .‬‬
‫‪ ‬ﻗﺿﻳﺏ ﺿﺎﻏﻁ ﻣﻌﺩﻧﻲ ﻳﺯﻥ )‪ (١٠ ± ٣٤٠‬ﺟﻡ ﻭﻗﻁﺭﻩ )‪ (٣± ٢٥‬ﻣﻡ‪.‬‬
‫‪ ‬ﺧﻁﻭﺍﺕ ﺍﻟﺗﺟﺭﺑﺔ ‪:‬‬
‫‪ .١‬ﻣﻠﺊ ﺍﻟـﺩﻭﺭﻕ ﺑﺎﻟﻣﻳﺎﻩ ﺣﺗﻲ ﺍﻟﻌﻼﻣﺔ ﺍﻟﻣﺣﺩﺩﺓ‪ ،‬ﻭﻭﺯﻥ ﺍﻟ ـﺩﻭﺭﻕ ﻭﻫ ﻭ ﻣﻣﺗﻠ ﺊ ﺑﺎﻟﻣ ﺎء‪ .‬ﻭﻟ ﻳﻛﻥ‬
‫)‪. ( B‬‬
‫‪ .٢‬ﺗﺟﻬﻳﺯ ﺣﻭﺍﻟﻲ ‪ ١٠٠٠‬ﺟﻡ ﻣﻥ ﺍﻟﺭﻛﻡ ﺍﻟﻧﺎﻋﻡ‪.‬‬
‫‪ .٣‬ﺗﺟﻔﻳﻑ ﺍﻟﻌﻳﻧﻪ ﻓﻲ ﺍﻟﻔﺭﻥ ﻋﻧﺩ )‪ (٥ ± ١١٠‬ﺩﺭﺟﺔ ﻣﺋﻭﻳﻪ ﺣﺗ ﻲ ﺗﺛﺑ ﺕ ﻭﺯﻧﻬ ﺎ‪ ،‬ﺗﺑ ﺭﺩ ﺍﻟﻌﻳﻧ ﻪ‬
‫ﺛﻡ ﺗﻐﻁﻲ ﺑﺎﻟﻣﻳﺎﻩ ﺍﻣﺎ ﺑﻐﻣﺭﻫﺎ ﺑﺎﻟﻣﻳﺎﻩ ﺍﻭ ﺍﺿﺎﻓﻪ ‪ %٦‬ﻋﻠﻲ ﺍﻻﻗﻝ ﻣﺎء ﻣﻥ ﻭﺯﻥ ﺍﻟﻌﻳﻧﻪ ﻟﻣﺩﻩ ‪ ‬‬
‫ﺻﻭﺭﻩ )‪ (١-٣‬ﺍﻻﺩﻭﺍﺕ ﺍﻟﻣﺳﺗﺧﺩﻣﻪ‬
‫)‪ (٤ ± ٢٤‬ﺳﺎﻋﺔ‪.‬‬
‫‪ .٤‬ﺍﺯﺍﻟﻪ ﺍﻟﻣﻳﺎﻩ ﺍﻟﺯﺍﺋﺩﻩ ﺑﺣﺭﺹ ﻟﺗﺟﻧﺏ ﻓﻘﺩ ﺍﻟﻣﻭﺍﺩ ﺍﻟﻧﺎﻋﻣﻪ‪ ،‬ﻓﺭﺩ ﺍﻟﻌﻳﻧﻪ ﻋﻠﻲ ﻟﻭﺡ ﺍﻣﻠﺱ ‪ ‬‬
‫ﻭﺗﻌﺭﺽ ﻟﻬﻭﺍء ﺩﺍﻓﺊ ﻟﺗﺟﻔﻳﻔﻬﺎ‪.‬‬
‫‪ .٥‬ﺗﺛﺑﻳﺕ ﺍﻟﻘﺎﻟﺏ ﻋﻠﻲ ﺳﻁﺢ ﺍﻣﻠﺱ‪ ،‬ﺑﺣﻳﺙ ﻳﻛﻭﻥ ﺍﻟﻘﻁﺭ ﺍﻻﻛﺑﺭ ﻣﻼﻣﺱ ﻟﻠﺳﻁﺢ‪  .‬‬
‫ﻭﺿﻊ ﺍﻟﻌﻳﻧﻪ ﻓﻲ ﺍﻟﻘﺎﻟﺏ ﺑﻛﺎﻣﻝ ﺳﻌﺗﻪ ﻭﺗﻛﺩﺱ ﺍﻟﻌﻳﻧﻪ ﺑﺎﻟﻳﺩ‪.‬‬
‫‪ .٦‬ﺩﻣﻙ ﺍﻟﻌﻳﻧﻪ ﻓﻲ ﺍﻟﻘﺎﻟﺏ ﺑـ ‪ ٢٥‬ﻁﺭﻗﻪ ﺑﺎﺳﺗﺧﺩﺍﻡ ﺍﻟﻘﺿ ﻳﺏ‪ .‬ﺍﺭﺗﻔ ﺎﻉ ﺳ ﻘﻭﻁ ﺍﻟﻘﺿ ﻳﺏ ﻓ ﻲ ﻛ ﻝ‬
‫ﻁﺭﻗﻪ ‪ ٥‬ﻣﻡ ﻣﻥ ﺳﻁﺢ ﺍﻟﻌﻳﻧﻪ‪ .‬ﺑﺣﻳﺙ ﺗﺳﻘﻁ ﺳﻘﻭﻁ ﺣﺭ ﺗﺣﺕ ﺗﺎﺛﻳﺭ ﻭﺯﻧﻪ‪.‬‬
‫‪ .٧‬ﺗﻧﻅﻳﻑ ﺣﻭﻝ ﺍﻟﻘﺎﻟﺏ‪ ،‬ﻭﻳﺭﻓﻊ ﺍﻟﻘﺎﻟﺏ ﺭﺍﺳﻳﺎ‪ .‬ﺍﺫﺍ ﺍﺣﺗﻔﻅﺕ ﺍﻟﻌﻳﻧﻪ ﺑﺷﻛﻝ ﺍﻟﻘﺎﻟﺏ ﻭﻟﻡ ﺗﻬﺑﻁ ﻳﺗﻡ‬
‫ﺗﻛﺭﺍﺭ ﺍﻟﺧﻁ ﻭﻩ ‪ ٦ ،٥ ،٤‬ﺣﺗ ﻲ ﻳﺣ ﺩﺙ ﻫﺑ ﻭﻁ ﻟﻠﻌﻳﻧ ﻪ ﻋﻧ ﺩ ﺭﻓ ﻊ ﺍﻟﻘﺎﻟ ﺏ ﻓﺗﻣﺛ ﻝ ﻫ ﺫﻩ ﺍﻟﺣﺎﻟ ﻪ‬
‫ﺍﻟﻌﻳﻧﻪ ﻣﺷﺑﻌﺔ ﺟﺎﻓﻪ ﺍﻟﺳﻁﺢ )‪.(S.S.D‬‬
‫‪ .٨‬ﻭﺯﻥ ﺣﻭﺍﻟﻲ )‪ (١٠ ± ٥٠٠‬ﺟﻡ ﻣﻥ ﺍﻟﻌﻳﻧﻪ ﺍﻟﻣﺷﺑﻌﻪ ﺟﺎﻓﺔ ﺍﻟﺳﻁﺢ ﻭﺗﺳ ﺟﻳﻝ ﺍﻟ ﻭﺯﻥ ﻭﻟ ﻳﻛﻥ‬
‫ﺻﻭﺭﻩ )‪ (٢-٣‬ﺗﻌﻳﻳﻥ ﻭﺯﻥ‬ ‫)‪.(S‬‬
‫‪ .٩‬ﺇﺿﺎﻓﻪ ﻣﺎء ﺍﻟﻲ ﺍﻟﺩﻭﺭﻕ ﻭﺍﺿﺎﻓﺔ ﺍﻟﻌﻳﻧﻪ ﺍﻟﻣﺷﺑﻌﺔ ﺟﺎﻓﻪ ﺍﻟﺳﻁﺢ )ﻭﺯﻧﻬﺎ ‪  ،(S‬‬
‫ﺍﻟﺩﻭﺭﻕ ﻭﺍﻟﻌﻳﻧﻪ ﻭﺍﻟﻣﺎء‬
‫ﻣﻠﺊ ﺣﻭﺍﻟﻲ ‪ %٩٠‬ﻣﻥ ﺳﻌﻪ ﺍﻟﺩﻭﺭﻕ‪ .‬ﻫﺯ ﺍﻟﻘﺎﻟﺏ ﺟﻳﺩﺍ ﻟﻠﺗﺧﻠﺹ ﻣﻥ ﺍﻟﻔﻘﺎﻗﻳﻊ ﺍﻟﻬﻭﺍﺋﻳﻪ‪.‬‬
‫ﻣﻠﺊ ﺍﻟﺩﻭﺭﻕ ﻟﻌﻼﻣﻪ ﺍﻟﻣﻌﺎﻳﺭﻩ‪.‬‬
‫‪ .١٠‬ﺗﻌﻳﻳﻥ ﻭﺯﻥ ﺍﻟﻌﻳﻧﻪ ﻭﺍﻟﺩﻭﺭﻕ ﻭﺍﻟﻣﻳﺎﻩ ﻭﻟﻳﻛﻥ )‪.(C‬ﺗﺟﻔﻳﻑ ﺍﻟﻌﻳﻧﻪ ﻓﻲ ﺍﻟﻔ ﺭﻥ ﻋﻧ ﺩ )‪ (١٠ ± ١١٠‬ﺩﺭﺟ ﻪ ﻣﺷ ﻭﻳﻪ ﺣﺗ ﻲ ﺗﺛﺑ ﺕ‬
‫ﻭﺯﻧﻬﺎ‪ .‬ﺗﻌﻳﻳﻳﻥ ﻭﺯﻥ ﺍﻟﻌﻳﻧﻪ ﺍﻟﺟﺎﻑ ﻭﻟﻳﻛﻥ )‪.(A‬‬
‫‪ ‬ﺍﻟﺗﺣﻠﻳﻝ ﻭ ﺍﻟﻧﺗﺎﺋﺞ ‪  :‬‬
‫‪ .١‬ﺣﺳﺎﺏ ﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ ﺍﻟﻛﻠﻲ ‪:‬‬
‫𝐴‬
‫𝑦𝑡𝑖𝑣𝑎𝑟𝐺 𝑐𝑖𝑓𝑖𝑐𝑒𝑝𝑆 𝑘𝑙𝑢𝐵‬ ‫‪ ‬‬
‫𝐵‬ ‫𝐶 𝑆‬
‫ﺣﻳﺙ ‪:‬‬
‫‪ :A‬ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ ﺍﻟﺟﺎﻓﻪ‪.‬‬
‫‪ :B‬ﻭﺯﻥ ﺍﻟﻌﻳﻧﻪ ﻣﺷﺑﻌﺔ ﺟﺎﻓﻪ ﺍﻟﺳﻁﺢ‪.‬‬
‫‪ :S‬ﻭﺯﻥ ﺍﻟﺩﻭﺭﻕ ﻭﻫﻭ ﻣﻣﺗﻠﺊ ﺑﺎﻟﻣﺎء‪.‬‬
‫ﺻﻭﺭﻩ )‪ (٣-٣‬ﺗﻌﻳﻳﻥ ﻭﺯﻥ ﺍﻟﻌﻳﻧﻪ‬
‫ﻣﺷﺑﻌﻪ ﻭﺟﺎﻓﻪ ﺍﻟﺳﻁﺢ‬ ‫‪ :C‬ﻭﺯﻥ ﺍﻟﺩﻭﺭﻕ ﻭﻫﻭ ﻣﻣﺗﻠﺊ ﺑﺎﻟﻌﻳﻧﻪ ﻭﺍﻟﻣﺎء‪  .‬‬
‫‪ .٢‬ﺣﺳﺎﺏ ﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ ﻣﺷﺑﻌﺔ ﺟﺎﻓﻪ ﺍﻟﺳﻁﺢ ‪:‬‬
‫𝐵‬
‫𝑦𝑡𝑖𝑣𝑎𝑟𝐺 𝑐𝑖𝑓𝑖𝑐𝑒𝑝𝑆 ‪𝑆. 𝑆. 𝐷.‬‬
‫𝐵‬ ‫𝐶 𝑆‬
‫‪ .٣‬ﺣﺳﺎﺏ ﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ ﺍﻟﻅﺎﻫﺭﻱ ‪:‬‬
‫𝐴‬
‫𝑦𝑡𝑖𝑣𝑎𝑟𝐺 𝑐𝑖𝑓𝑖𝑐𝑒𝑝𝑆 𝑡𝑛𝑒𝑟𝑎𝑝𝑝𝐴‬
‫𝐴‬ ‫𝐶 𝑆‬
‫‪ .٤‬ﻧﺳﺑﻪ ﺍﻣﺗﺻﺎﺹ ﺍﻟﻣﻳﺎﻩ ‪:%‬‬
‫𝐴 𝑆‬
‫‪𝑊𝑎𝑡𝑒𝑟 𝐴𝑏𝑠𝑜𝑟𝑝𝑡𝑖𝑜𝑛 %‬‬
‫𝐴‬
‫‪ ‬ﺍﻟﺗﻘﺭﻳﺭ ‪  :‬‬
‫‪ .١‬ﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ ﺍﻟﻛﻠﻲ‪.‬‬
‫‪ .٢‬ﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ ﺍﻟﻛﻠﻲ )ﻣﺷﺑﻌﺔ ﺟﻔﻪ ﺍﻟﺳﻁﺢ(‪.‬‬
‫‪ .٣‬ﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ ﺍﻟﻅﺎﻫﺭﻱ‪.‬‬
‫‪ .٤‬ﺍﻻﻣﺗﺻﺎﺹ‪.‬‬
‫‪ ‬‬
Specific Gravity Test of Fine Aggregate
 

Wt. of Pyconometer& Water  S =    gm 


S.S.D Weight  B =    gm 
Wt. of Pyconometer& Water & Sample  C =    gm 
Weight in Air  A =    gm 

Specific Gravity Values:
Bulk Specific Gravity  =  A/(B+S‐C)   
  =    gm/cm3 
S.S.D Specific Gravity  =  B/(B+S‐C)   
  =    gm/cm3 
Apparent Specific Gravity  =  A/(A+S‐C)   
  =    gm/cm3 

Water Absorption % 
Water Absorption   =  (S‐A)/A   
  =    % 

 
‫ﺗﺟﺭﺑﺔ ‪-٤-‬‬
‫ﺍﺧﺗﺑﺎﺭ ﻟﻭﺱ ﺍﻧﺟﻠﻭﺱ‬
‫‪  Resistance to Degradation of small‐size Coarse Aggregate ‬‬
‫‪  by Abrasion and Impact in the Los Angeles Machine‬‬
‫‪ASTM C131 – 01‬‬
‫‪ ‬ﺍﻟﻐﺭﺽ ‪:‬‬
‫ﻻﺧﺗﺑﺎﺭ ﻣﻘﺎﻭﻣﺔ ﺍﻟﺭﻛﺎﻡ ﺍﻟﺧﺷﻥ ﺍﻻﻗﻝ ﻣﻥ ‪ ٣٧٫٥‬ﻣﻡ ﻟﻠﺑﺭﻱ‪ ،‬ﺍﻻﺣﺗﻛﺎﻙ ﻭ ﺍﻟﺻﺩﻡ ﺑﺎﺳﺗﺧﺩﺍﻡ ﺟﻬﺎﺯ ﻟﻭﺱ ﺍﻧﺟﻠﻭﺱ‪.‬‬
‫‪ ‬ﺍﻻﻫﻣﻳﺔ ﻭﺍﻻﺳﺗﺧﺩﺍﻡ ‪  :‬‬
‫ﺍﻟﺗﺎﻛﺩ ﻣﻥ ﻣﻘﺎﻭﻣﻪ ﺍﻟﺭﻛﺎﻡ ﻟﻠﺑﺭﻱ ﻭﺍﻻﺣﺗﻛﺎﻙ‪.‬‬
‫ﺍﻻﺟﻬﺯﺓ ﺍﻟﻣﺳﺗﺧﺩﻣﺔ ‪  :‬‬ ‫‪‬‬
‫ﺟﻬﺎﺯ ﻟﻭﺱ ﺍﻧﺟﻠﻭﺱ‪ .‬ﻋﺑﺎﺭﺓ ﻋﻥ ﺍﺳﻁﻭﺍﻧﺔ ﻣﻔﺭﻏﻪ ﻳﺑﻠﻎ ﻗﻁﺭﻫﺎ ﺍﻟﺩﺍﺧﻠﻲ ‪ ٥٠٨‬ﻣ ﻡ‬ ‫‪‬‬
‫ﻭﻁﻭﻟﻪ ‪ ٧١١‬ﻣﻡ‪ ،‬ﻭﻣﺯﻭﺩ ﺑﻔﺗﺣﻪ ﻹﺩﺧﺎﻝ ﻭﺗﻔﺭﻳﻎ ﺍﻟﻌﻳﻧﺔ‪ ،‬ﺷﻛﻝ )‪  .(١-٤‬‬
‫ﻣﻧﺎﺧﻝ‪.‬‬ ‫‪‬‬
‫ﻣﻳﺯﺍﻥ ﺩﻗﺗﻪ ‪ %٠٬١‬ﻣﻥ ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ‪.‬‬ ‫‪‬‬
‫ﻣﺟﻣﻭﻋﺔ ﻣﻥ ﺍﻟﻛﺭﺍﺕ ﺍﻟﻣﻌﺩﻧﻳﺔ )ﻳﺑﻠﻎ ﻗﻁﺭﻫﺎ ‪ ٤٦٬٨‬ﻣﻡ ﺗﻘﺭﻳﺑﺎ ﻭﺗﺯﻥ ‪ ٤٢٠‬ﺟﻡ(‪.‬‬ ‫‪‬‬
‫ﻳﻌﺗﻣﺩ ﻋﺩﺩ ﺍﻟﻛﺭﺍﺕ ﺍﻟﻣﻌﺩﻧﻳﺔ ﻋﻠﻲ ﺗﺩﺭﺝ ﻋﻳﻧﺔ ﺍﻻﺧﺗﺑﺎﺭ‪  ....‬‬
‫ﺍﻟﻭﺯﻥ)ﺟﻡ(‬ ‫ﻋﺩﺩ ﺍﻟﻛﺭﺍﺕ‬ ‫ﺍﻟﺗﺩﺭﺝ‬ ‫‪ ‬‬
‫‪٢٥ ± ٥٠٠٠‬‬ ‫‪ ‬‬
‫‪12‬‬ ‫‪ A‬‬
‫‪ ‬‬
‫‪  ٢٥ ± ٤٥٨٤‬‬ ‫‪11‬‬ ‫‪B‬‬
‫‪ ‬‬
‫‪٢٠ ± ٣٣٣٠‬‬ ‫‪8‬‬ ‫‪C‬‬
‫‪١٥ ± ٢٥٠٠‬‬ ‫‪6‬‬ ‫‪D‬‬ ‫‪ ‬‬

‫ﺷﻛﻝ )‪ (١-٤‬ﺟﻬﺎﺯ ﻟﻭﺱ ﺍﻧﺟﻠﻭﺱ ‪ ‬‬ ‫‪ ‬ﺗﺟﻬﻳﺯ ﺍﻟﻌﻳﻧﺔ ‪:‬‬


‫ﺣﺭﺍﺭﺓ )‪ (٥ ± ١١٠‬ﺩﺭﺟﺔ ﻣﺋﻭﻳﺔ‬ ‫‪ .١‬ﻏﺳﻝ ﺍﻟﺭﻛﺎﻡ ﺟﻳﺎ ﻭﺗﺟﻔﻳﻔﻬﺎ ﻋﻧﺩ ﺩﺭﺟﺔ‬
‫ﺣﺗﻲ ﻳﺛﺑﺕ ﻭﺯﻧﻬﺎ‪ .‬ﺗﺧﻠﻁ ﺍﻟﻌﻳﻧﺔ ﺑﺎﻟﻛﻣﻳﺎﺕ ﺍﻟﻣﻭﺿﺣﺔ ﺑﺎﻟﺟﺩﻭﻝ ‪،.... ١‬‬
‫ﺍﻟﺗﺩﺭﺝ‬
‫ﺍﻟﻣﺣﺟﻭﺯ‬ ‫ﺍﻟﻣﺎﺭ‬
‫‪D‬‬ ‫‪C‬‬ ‫‪B‬‬ ‫‪ A‬‬
‫‪٢٥ ± ١٢٥٠‬‬ ‫‪٢٥‬‬ ‫‪٣٧٬٥‬‬
‫‪٢٥ ± ١٢٥٠‬‬ ‫‪١٩‬‬ ‫‪٢٥‬‬
‫‪١٠ ± ٢٥٠٠‬‬ ‫‪١٠ ± ١٢٥٠‬‬ ‫‪١٢٬٥‬‬ ‫‪١٩‬‬
‫‪١٠ ± ٢٥٠٠‬‬ ‫‪١٠ ± ١٢٥٠‬‬ ‫‪٩٬٥‬‬ ‫‪١٢٬٥‬‬
‫‪١٠ ± ٢٥٠٠‬‬ ‫‪٦٬٣‬‬ ‫‪٩٬٥‬‬
‫‪١٠ ± ٢٥٠٠‬‬ ‫‪٤٬٧٥‬‬ ‫‪٦٬٣‬‬
‫‪١٠ ± ٥٠٠٠‬‬ ‫‪٢٬٣٦‬‬ ‫‪٤٬٧٥‬‬
‫‪١٠ ± ٥٠٠٠‬‬ ‫‪١٠ ± ٥٠٠٠‬‬ ‫‪١٠ ± ٥٠٠٠‬‬ ‫‪١٠ ± ٥٠٠٠‬‬ ‫ﺍﻟﻣﺟﻣﻭﻉ‬
‫‪ ‬‬
‫‪ ‬‬
‫‪ .٢‬ﻭﺿﻊ ﺍﻟﻌﻳﻧﺔ ﻭﺍﻟﻛﺭﺍﺕ ﺍﻟﻣﻌﺩﻧﻳﺔ ﻓﻲ ﺟﻬﺎﺯ ﻟﻭﺱ ﺍﻧﺟﻠﻭﺱ ﻭﺗﺷﻐﻳﻝ ﺍﻟﺟﻬﺎﺯ ﺑﺳﺭﻋﺔ )‪ (٣٣ : ٣٠‬ﻟﻔﺔ ﻓﻲ ﺍﻟﺩﻗﻳﻘﺔ ﺣﺗﻲ ‪ ٥٠٠‬ﻟﻔﺔ‪.‬‬
‫‪ .٣‬ﺇﺧﺭﺍﺝ ﺍﻟﻌﻳﻧﺔ ﻣﻥ ﺍﻟﺟﻬﺎﺯ ﻭﻓﺻﻠﻬﺎ ﻋﻠﻲ ﻣﻧﺧﻝ ﺍﺧﺷﻥ ﻣﻥ )‪ ١٬٧‬ﻣﻡ( ﺭﻗﻡ ‪.١٢‬‬
‫‪ .٤‬ﻏﺳﻝ ﺍﻟﻣﻭﺍﺩ ﺍﻻﺧﺷﻥ ﻣﻥ ‪ ١٬٧‬ﻣﻡ‪ ،‬ﻭﺗﺟﻔﻳﻔﻬﺎ ﻋﻧﺩ ﺩﺭﺟﺔ ﺣﺭﺍﺭﺓ )‪ (٥ ± ١١٠‬ﺩﺭﺟﺔ ﻣﺋﻭﻳﺔ ﺣﺗﻲ ﻳﺛﺑﺕ ﻭﺯﻧﻬﺎ‪ .‬ﻭﺣﺳﺏ ﺍﻟﻭﺯﻥ‬
‫ﻷﻗﺭﺏ ‪ ١‬ﺟﻡ‪  .‬‬
‫‪ ‬ﺍﻟﻧﺗﺎﺋﺞ ‪  :‬‬
‫‪ ‬ﺣﺳﺎﺏ ﻧﺳﺑﺔ ﺍﻟﻔﺎﻗﺩ ﻓﻲ ﺍﻟﻣﻭﺍﺩ ﻧﺗﻳﺟﺔ ﺍﻟﺑﺭﻱ ﻭﺍﻻﺣﺗﻛﺎﻙ‬
‫‪W‬‬ ‫‪W‬‬
‫‪% Losses‬‬ ‫‪x100‬‬
‫‪W‬‬
‫ﺣﻳﺙ ‪  :‬‬
‫‪:% Losses‬ﻧﺳﺑﺔ ﺍﻟﻔﺎﻗﺩ ﻓﻲ ﺍﻟﻣﻭﺍﺩ ﻧﺗﻳﺟﺔ ﺍﻻﺣﺗﻛﺎﻙ ﻭﺍﻟﺑﺭﻱ‪.‬‬
‫‪ :Wo‬ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ ﻗﺑﻝ ﺍﻻﺧﺗﺑﺎﺭ ﻷﻗﺭﺏ‪ ١ ،‬ﺟﻡ‪.‬‬
‫‪ :W1‬ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ ﺍﻟﻣﺎﺭ ﻣﻥ ﺍﻟﻣﻧﺧﻝ ‪ ١٢#‬ﻷﻗﺭﺏ‪ ١ ،‬ﺟﻡ‪.‬‬
‫‪ ‬ﺍﻟﺗﻘﺭﻳﺭ ‪  :‬‬
‫ﻣﺻﺩﺭ ﺍﻟﺭﻛﺎﻡ‪ ،‬ﻧﻭﻋﻪ ﻭﺍﻟﻣﻘﺎﺱ ﺍﻻﻋﺗﺑﺎﺭﻱ ﺍﻻﻛﺑﺭ )‪.(Nominal Aggregate Max. Size‬‬
‫ﺍﻟﺗﺩﺭﺝ ﺍﻟﻣﺳﺗﺧﺩﻡ ﻟﻼﺧﺗﺑﺎﺭ‪ ،‬ﺟﺩﻭﻝ ‪.١‬‬
‫ﺍﻟﻔﺎﻗﺩ ﻓﻲ ﺍﻟﻣﻭﺍﺩ ﻧﺗﻳﺟﺔ ﺍﻟﺑﺭﻱ ﻭﺍﻻﺣﺗﻛﺎﻙ ﻭﺍﻟﺻﺩﻡ ﻷﻗﺭﺏ ‪ % ١‬ﻣﻥ ﺍﻟﻭﺯﻥ‪.‬‬
‫‪ ‬‬ ‫‪ ‬‬
  Los Angeles Test
 
  Type of Gradation 
Gradation
Passing Retain
 
37.5  25 
25  19 
19  12.5 
12.5  9.5 
9.5  6.3 
6.3  4.75 
4.75  2.36
Sum 
 

  Calculations
Nominal Aggregate Max. Size  =   mm
Initial Weight    Wo = gm
Retaining Wt. on Sieve #12 After 500 Rev.    W2 = gm
Passing Wt. from sieve #12 After 500 Rev.   W1 = Wo – W2
 = gm
𝑊
% Abrasion  = 𝑊
 =   %
 `

   
‫ﺗﺟﺭﺑﺔ ﺭﻗﻡ ‪-6-‬‬
‫ﺍﺧﺗﺑﺎﺭ ﺍﻟﻣﻛﺎﻓﺊ ﺍﻟﺭﻣﻠﻲ ﻟﻠﺗﺭﺑﻪ ﻭﺍﻟﺭﻛﺎﻡ ﺍﻟﻧﺎﻋﻡ‬
‫‪  Sand Equivalent Value of Soil and Fine Aggregate‬‬
‫‪  ASTM D2419‬‬
‫‪ ‬ﺍﻟﻐﺭﺽ ‪:‬‬
‫ﺗﻌﻳﻳﻥ ﻧﺳﺑﻪ ﺍﻟﻁﻳﻥ ﺍﻭ ﻧﺳﺑﻪ ﺍﻟﻣﻭﺍﺩ ﺍﻟﻧﺎﻋﻣﻪ ﺍﻟﻠﺩﻧﻪ ﻓﻲ ﺍﻟﺗﺭﺑﻪ ﻭﺍﻟﺭﻛﺎﻡ ﺍﻟﻧﺎﻋﻡ ﺍﻟﻣﺎﺭ ﻣﻥ ﺍﻟﻣﻧﺧﻝ ﺭﻗﻡ ‪.٤‬‬
‫‪ ‬ﺍﻻﻫﻣﻳﺔ ﻭﺍﻻﺳﺗﺧﺩﺍﻡ ‪:‬‬
‫ﻳﺳﺗﺧﺩﻡ ﻫﺫﺍ ﺍﻻﺧﺗﺑﺎﺭ ﻓﻲ ﺗﻌﻳﻥ ﻗﻳﻣﻪ ﺗﺟﺭﻳﺑﻳﻪ ﻟﻧﺳﺑﻪ ﻭﺧﺻﺎﺋﺹ ﺍﻟﻁﻳﻥ ﺍﻟﻣﻭﺟﻭﺩﻩ ﻓﻲ ﻋﻳﻧﻪ ﺍﻻﺧﺗﺑﺎﺭ‪.‬‬
‫‪ ‬ﺍﻻﺟﻬﺯﻩ‪:‬‬
‫ﻣﺧﺑﺎﺭ ﻣﺩﺭﺝ‪ ،‬ﺳﺩﺍﺩﻩ ﻣﻁﺎﻁﻳﻪ‪ ،‬ﺍﻧﺑﻭﺑﻪ‪ ،‬ﺛﻘﻝ ﻭﺳﻳﻔﻭﻥ ﺷﻛﻝ )‪.(١-٦‬‬
‫ﻣﻧﺧﻝ ‪ ٤٫٧٥‬ﻣﻡ )‪ (٤#‬ﻟﻔﺻﻝ ﺍﻟﻣﻭﺍﺩ ﺍﻟﻧﺎﻋﻣﻪ‪.‬‬
‫ﺍﺳﻁﻭﺍﻧﻪ ﻗﻁﺭﻫﺎ ‪ ٥٧‬ﻣﻡ ﻭﺳﻌﺗﻬﺎ ‪ ٥ ± ٨٥‬ﻣﻠﻲ ﻟﺗﺭ‪.‬‬
‫ﻗﻣﻊ‪.‬‬
‫ﻓﺭﻥ ﻗﺎﺩﺭ ﻟﻠﺣﻔﺎﻅ ﻋﻠﻲ ﺩﺭﺟﻪ ﺍﻟﺣﺭﺍﺭﻩ ﻋﻧﺩ )‪ (٥ ± ١١٠‬ﺩﺭﺟﻪ ﻣﺋﻭﻳﻪ‪.‬‬
‫‪ ‬ﺧﻁﻭﺍﺕ ﺍﻟﺗﺟﺭﺑﻪ‪:‬‬
‫‪ .١‬ﺇﺿﺎﻓﺔ ﻣﺣﻠﻭﻝ ﻛﻠﻭﺭﻳﺩ ﺍﻟﻛﺎﻟﺳﻳﻭﻡ ﻓﻲ ﺍﻟﺳﻳﻔﻭﻥ ﻟﻠﻌﻼﻣﺔ ‪ ٠٫١ ± ٤‬ﺑﻭﺻﻪ )‪ ٣ ± ١٠٢‬ﻣﻡ(‪  .‬‬
‫‪ .٢‬ﺻﺏ ﺍﻟﻌﻳﻧﺔ ﻓﻲ ﺍﻟﻣﺧﺑﺎﺭ ﺑﺎﺳﺗﺧﺩﺍﻡ ﻗﻣﻊ ﻟﺗﺟﻧﺏ ﺗﺳﺭﺏ ﺍﻟﻌﻳﻧﺔ‪  .‬‬
‫‪ .٣‬ﻗﺭﻉ ﻣﺅﺧﺭﻩ ﺍﻟﻣﺧﺑﺎﺭ ﺑﻭﺳﻁﻪ ﺍﻟﻳﺩ ﻋﺩﻩ ﻣﺭﺍﺕ ﻹﺧﺭﺍﺝ ﺍﻟﻔﻘﺎﻗﻳﻊ ﺍﻟﻬﻭﺍﺋﻳﺔ‪  .‬‬
‫‪ .٤‬ﺗﺭﻙ ﺍﻟﻌﻳﻧﺔ ﺍﻟﻣﺑﻠﻠﺔ ﻭﺍﻟﻣﺧﺑﺎﺭ ﻟﻣﺩﻩ ‪ ١ ± ١٠‬ﺩﻗﻳﻘﻪ‪  .‬‬

‫ﻋﻠ ﻲ ﻓﻭﻫ ﻪ ﺍﻟﻣﺧﺑ ﺎﺭ‪ ،‬ﻗﻠ ﺏ‬ ‫ﺷﻛﻝ )‪ (١-٦‬ﺍﻻﺩﻭﺍﺕ ﺍﻟﻣﺳﺗﺧﺩﻣﻪ ‪ ‬‬ ‫‪ .٥‬ﺑﻌ ﺩ ﻓﺗ ﺭﻩ ﺍﻟﺑﻠ ﻝ )‪ ١٠‬ﺩﻗ ﺎﺋﻖ( ﺿ ﻊ ﺍﻟﺳ ﺩﺍﺩﺓ ﺍﻟﻣﻁﺎﻁﻳ ﺔ‬
‫ﺍﻟﻣﺧﺑﺎﺭ ﻭﺭﺟﻬﺎ ﻟﺗﻔﻛﻳﻙ ﺣﺑﻳﺑﺎﺕ ﺍﻟﻌﻳﻧﺔ‪  .‬‬
‫‪ .٦‬ﺑﺎﺳﺗﺧﺩﺍﻡ ﺍﻟﻬﺯ ﺍﻟﻳﺩﻭﻱ‪  :‬‬
‫‪ .٦٫١‬ﻣﺳﻙ ﺍﻟﻣﺧﺑﺎﺭ ﻓﻲ ﺍﻟﻭﺿﻊ ﺍﻻﻓﻘﻲ ﻛﻣﺎ ﻫﻭ ﻣﻭﺿﻊ ﻓﻲ ﻭﻫﺯ ﺍﻟﻣﺧﺑﺎﺭ ﻓﻲ ﺣﺭﻛﻪ ﺍﻓﻘﻳﻪ ﻣﻥ ﺍﻟﻧﻬﺎﻳﺔ ﺍﻟﻲ ﺍﻟﻧﻬﺎﻳﺔ‪  .‬‬
‫‪ .٦٫٢‬ﻫﺯ ﺍﻟﻣﺧﺑﺎﺭ ‪ ٩٠‬ﺩﻭﺭﻩ ﺧﻼﻝ ‪ ٣٠‬ﺛﺎﻧﻳﻪ ﺗﻘﺭﻳﺑﺎ‪  .‬‬
‫‪ .٧‬ﻋﻣﻠﻳﻪ ﺍﻟﺳﻘﻲ ‪  Irrigation Procedure‬‬
‫‪ -٧٫١‬ﻭﺿﻊ ﺍﻟﻣﺧﺑﺎﺭ ﺭﺍﺳﻳﺎ ً ﺍﺛﻧﺎء ﻋﻣﻠﻳﻪ ﺍﻟﺳﻘﻲ‪ ،‬ﺷﻁﻑ ﺍﻟﻣﻭﺍﺩ ﺍﻟﻧﺎﻋﻣﺔ ﺍﻟﻌﺎﻟﻘﺔ ﻋﻠﻲ ﺟﺩﺭﺍﻥ ﺍﻟﻣﺧﺑﺎﺭ ﺑﺳﺑﺏ ﺍﻟﻬﺯ‪  ،‬‬
‫‪ -٧٫٢‬ﻏﺭﺯ ﺍﻟـ ـ ‪Irrigator‬ﺧ ﻼﻝ ﺍﻟﻌﻳﻧ ﺔ ﻟﻘ ﺎﻉ ﺍﻟﻣﺧﺑ ﺎﺭ )ﺑﺣﻳ ﺙ ﻳﻛ ﻭﻥ ﺍﻻﺧﺗ ﺭﺍﻕ ﺑﺭﻓ ﻖ ﻣﺻ ﺎﺣﺏ ﻻﻟﺗ ﻭﺍء ﻭﻳﻛ ﻭﻥ‬
‫ﺍﻟﻣﺣﻠﻭﻝ ﻣﺗﺩﻓﻖ ﻣﻥ ﻓﻭﻫﻪ ﺍﻷﻧﺑﻭﺑﺔ(‪ .‬ﻟﺟﻌﻝ ﺍﻟﻣﻭﺍﺩ ﺍﻟﻧﺎﻋﻣﺔ ﻋﺎﻟﻘﺔ ﻓﻭﻕ ﺣﺑﻳﺑﺎﺕ ﺍﻟﺭﻣﻝ ﺍﻟﺧﺷﻧﺔ‪  .‬‬
‫‪ -٧٫٣‬ﺍﺳﺗﻣﺭﺍﺭ ﺍﻟﺧﻁﻭﺓ ﺍﻟﺳﺎﺑﻘﺔ ﺣﺗﻲ ﻳﻘﺗﺭﺏ ﺍﻟﻣﺣﻠﻭﻝ ﻣ ﻥ ﺍﻟﻌﻼﻣ ﺔ ‪ ١٥‬ﺑﻭﺻ ﻪ )‪ ٣٨‬ﺳ ﻡ(‪ ،‬ﺛ ﻡ ﺗﺭﻓ ﻊ ﺍﻷﻧﺑﻭﺑ ﺔ ﺑ ﺑﻁء‬
‫ﻣﻊ ﺍﺳﺗﻣﺭﺍﺭ ﺗﺩﻓﻖ ﺍﻟﻣﺣﻠﻭﻝ ﻣﻥ ﻓﻭﻫﻪ ﺍﻻﻧﺑﻭﺑﺔ ﺣﺗﻲ ﻳﺻﻝ ﺍﻟﻣﺣﻠﻭﻝ ﻟﻠﻌﻼﻣﺔ ‪ ١٥‬ﺑﻭﺻﻪ‪  .‬‬
‫‪ .٨‬ﺗﺭﻙ ﺍﻟﻣﺧﺑﺎﺭ ﻭﺍﻟﻌﻳﻧﺔ ﻟﻣﺩﻩ ‪ ٢٠‬ﺩﻗﻳﻘﺔ ‪ ١٥ ±‬ﺛﺎﻧﻳﻪ‪  .‬‬
‫‪ .٩‬ﺑﻌﺩ ﺍﻧﺗﻬﺎء ﻓﺗﺭﻩ ﺍﻟﺗﺭﺳﻳﺏ )‪ ٢٠‬ﺩﻗﻳﻘﻪ(‪ ،‬ﻳﺗﻡ ﺗﺳﺟﻳﻝ ﻣﻧﺳﻭﺏ ﺍﻟﻁﻳﻥ ﺍﻟﻣﻌﻠﻖ‪ ،‬ﺇﺫﺍ ﻟﻡ ﻳﻛﻥ ﺣﺩﻭﺩ ﺍﻟﻁﻳﻥ ﻭﺍﺿﺣﻪ ﻟﻠﻘﺭﺍءﺓ ﺑﻌﺩ ﻓﺗ ﺭﻩ‬
‫ﺍﻟﺗﺭﺳﻳﺏ ﺗﺗﺭﻙ ﺍﻟﻌﻳﻧﺔ ﻟﻠﺣﺻﻭﻝ ﻋﻠﻲ ﻗﺭﺍءﻩ ﻭﺍﺿﺣﻪ ﻟﻠﻁ ﻳﻥ ﻭﺇﺫﺍ ﻛ ﺎﻥ ﻓﺗ ﺭﻩ ﺍﻟﺗﺭﺳ ﻳﺏ ﺍﻛﺑ ﺭ ﻣ ﻥ ‪ ٣٠‬ﺩﻗﻳﻘ ﻪ ﺗُﻌ ﺎﺩ ﺍﻟﺗﺟﺭﺑ ﺔ ﻣ ﻥ‬
‫ﺟﺩﻳﺩ ﻋﻠﻲ ‪ ٣‬ﻋﻳﻧﺎﺕ ﻣﻥ ﻧﻔﺱ ﺍﻟﻣﺎﺩﺓ‪  .‬‬
‫‪ .١٠‬ﺗﺣﺩﻳﺩ ﻣﻧﺳﻭﺏ ﺍﻟﺭﻣﻝ‪  Sand Reading Determination    ‬‬
‫‪ -١٠٫١‬ﺑﻌ ﺩ ﻗ ﺭﺍءﺓ ﻣﻧﺳ ﻭﺏ ﺍﻟﻁ ﻳﻥ‪ ،‬ﻳ ﺗﻡ ﻭﺿ ﻊ ﺍﻟﺛﻘ ﻝ ﻭﺇﻧﺯﺍﻟ ﻪ ﺑﺭﻓ ﻖ ﺣﺗ ﻲ ﻳﺳ ﺗﻘﺭ ﻋﻠ ﻲ‬
‫ﺍﻟﺭﻣﻝ‪ ،‬ﻭﻋﺩﻡ ﺳﻣﺎﺡ ﺍﻟﻣﺅﺷﺭ ﺍﻥ ﻳﺻﻁﺩﻡ ﺑﻔﻭﻫﻪ ﺍﻻﺳﻁﻭﺍﻧﺔ ﻋﻧﺩ ﺇﻧﺯﺍﻝ ﺍﻟﺛﻘﻝ‪  .‬‬
‫‪ -١٠٫٢‬ﻋﻧ ﺩ ﺍﻗﺗ ﺭﺍﺏ ﺍﻟﺛﻘ ﻝ ﻣ ﻥ ﺍﻟﺭﻣ ﻝ ﻳ ﺗﻡ ﺍﻣﺎﻟ ﻪ ﺭﺍﺱ ﺍﻟﺛﻘ ﻝ ﺗﺟ ﺎﻩ ﺍﻟﻣﺧﺑ ﺎﺭ ﺣﺗ ﻲ ﻳﻠﻣ ﺱ‬
‫ﺍﻟﻣﺅﺷ ﺭ ﺍﻟﻣﺧﺑ ﺎﺭ‪ ،‬ﻳ ﺗﻡ ﻁ ﺭﺡ ﺍﻟﻣﻧﺳ ﻭﺏ ﻣ ﻥ ‪ ١٠‬ﺑﻭﺻ ﺔ )‪ ٢٥٫٤‬ﺳ ﻡ( ﻟﻳﻌﻁ ﻲ‬
‫ﻣﻧﺳﻭﺏ ﺍﻟﺭﻣﻝ‪  .‬‬
‫‪ -١٠٫٣‬ﻳﺟﺏ ﺍﻟﺗﺄﻛﺩ ﻣﻥ ﻋﺩﻡ ﺍﺧﺗﺭﻕ ﺍﻟﺛﻘﻝ ﻟﻁﺑﻘﻪ ﺍﻟﺭﻣﻝ ﻗﺑﻝ ﺗﺳﺟﻳﻝ ﺍﻟﻘﺭﺍءﺓ‪  .‬‬
‫ﻳﺗﻡ ﺗﻘﺭﻳﺏ ﻣﻧﺳﻭﺏ ﺍﻟﻁﻳﻥ ﻭﺍﻟﺭﻣﻝ ﻷﻗﺭﺏ ‪ ٠٬١‬ﺑﻭﺻﻪ )‪ ٢٬٥‬ﻣﻡ(‪  .‬‬ ‫‪‬‬
‫‪ ‬ﺍﻟﻧﺗﺎﺋﺞ‪  :‬‬
‫ﻗﺭﺍءﻩ ﺍﻟﺭﻣﻝ‬
‫ﺍﻟﻣﻛﺎﻓﺊ ﺍﻟﺭﻣﻠﻲ=‬ ‫‪x ١٠٠‬‬
‫ﻗﺭﺍءﻩ ﺍﻟﻁﻳﻥ‬
‫‪ ‬ﻳﺗﻡ ﺗﻘﺭﻳﺏ ﺍﻟﻣﻛﺎﻓﺊ ﺍﻟﺭﻣﻠﻲ ﻷﻛﺑﺭ ﺭﻗﻡ ﺻﺣﻳﺢ‪  .‬‬
‫‪ ‬‬

‫ﺷﻛﻝ )‪ (٢-٦‬ﻗﺭﺍءﻩ ﺍﺭﺗﻔﺎﻉ ﺍﻟﺭﻣﻝ ﺑﺎﺳﺗﺧﺩﻣﻪ ﺍﻟﺛﻘﻝ ‪ ‬‬

‫ﺷﻛﻝ )‪ (٣-٦‬ﺍﻟﻘﺭﺍءﺍﺕ‬
‫ﺗﺟﺭﺑﺔ ﺭﻗﻡ ‪-٧-‬‬
‫ﺍﻻﺧﺗﺑﺎﺭ ﺍﻟﻘﻳﺎﺳﻲ ﻟﻣﺗﺎﻧﺔ ﺍﻟﺭﻛﺎﻡ ﻭﺗﺣﻣﻠﻪ ﺍﻟﻌﻭﺍﻣﻝ ﺍﻟﺑﻳﺋﻳﺔ )ﺍﻟﺗﺟﻣﺩ ﻭﺍﻻﻧﺻﻬﺎﺭ( ﺑﺎﺳﺗﺧﺩﺍﻡ ﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﺻﻭﺩﻳﻭﻡ ﻭﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﻣﺎﻏﻧﺳﻳﻭﻡ‬
‫‪  Standard Test Method for Soundness of Aggregates‬‬
‫‪  by use of Sodium Sulfate or Magnesium Sulfate‬‬
‫‪ASTM C88‐99a ‬‬

‫‪ ‬ﺍﻟﻐﺭﺽ‪  :‬‬
‫ﻫ ﺫﺍ ﺍﻻﺧﺗﺑ ﺎﺭ ﻳﺳ ﺗﺧﺩﻡ ﻓ ﻲ ﻣﻌﺭﻓ ﺔ ﻣﺗﺎﻧ ﺔ ﺍﻟﺭﻛ ﺎﻡ ﻭﻣ ﺩﻯ ﻗﺩﺭﺗ ﻪ ﻋﻠ ﻰ ﺗﺣﻣ ﻝ ﺍﻟﻌﻭﺍﻣ ﻝ ﺍﻟﺟﻭﻳ ﺔ ﺍﻟﻣﺣﻳﻁ ﺔ ﺑ ﻪ ﻭﺍﻟﻣﺗﻐﻳ ﺭﺓ ﻣ ﻥ ﺗﺟﻣ ﺩ‬
‫ﻭﺍﻧﺻﻬﺎﺭ ﻋﻥ ﻁﺭﻳﻖ ﺍﻟﻐﻣﺭ ﻣﺭﺍﺕ ﻋﺩﻳﺩﺓ ﻓﻲ ﻣﺣﻠﻭﻝ ﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﺻﻭﺩﻳﻭﻡ ﺍﻭ ﻣﺣﻠﻭﻝ ﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﻣﺎﻏﻧﺳﻳﻭﻡ ﺣﺗﻰ ﻳﺻ ﻝ ﺍﻟ ﻰ ﺩﺭﺟ ﺔ‬
‫ﺍﻟﺗﺷﺑﻊ ﻓﻲ ﻛﻝ ﺩﻭﺭﺓ ﺛﻡ ﺍﻟﺗﺟﻔﻳﻑ ﻭﺇﻋﺎﺩﺓ ﺍﻟﻐﻣﺭ ﻣﺭﺓ ﺃﺧﺭﻯ‪.‬‬
‫ﻓﻲ ﻫﺫﺍ ﺍﻻﺧﺗﺑﺎﺭ ﺗﻘﻭﻡ ﻗﻭﻯ ﺍﻟﺗﻣ ﺩﺩ ﺍﻟﺩﺍﺧﻠﻳ ﺔ ﺍﻟﻘﺎﺩﻣ ﺔ ﻣ ﻥ ﺩﻭﺭﺍﺕ ﺍﻟﻐﻣ ﺭ ﻭﺍﻟﺗﺟﻔﻳ ﻑ ﺑﻌﻣ ﻝ ﻣﺣﺎﻛ ﺎﺓ ﺑ ﻳﻥ ﺩﻭﺭﺍﺕ ﺍﻟﺗﺟﻣ ﺩ ﻭﺍﻻﻧﺻ ﻬﺎﺭ‬
‫ﺍﻟﺫﻱ ﻳﺣﺩﺙ ﻟﻠﺭﻛﺎﻡ ﻧﺗﻳﺟﺔ ﺍﻟﻌﻭﺍﻣﻝ ﺍﻟﺟﻭﻳﺔ ﺍﻟﻣﺣﻳﻁﺔ ﺑﺎﻟﺭﻛﺎﻣﺣﻳ ﺙ ﺗﻘ ﻭﻡ ﺑﻠ ﻭﺭﺍﺕ ﺍﻻﻣ ﻼﺡ ﺩﺍﺧ ﻝ ﺍﻟﺭﻛ ﺎﻡ ﺑﻣﺣﺎﻛ ﺎﺓ ﺍﻟﺿ ﻐﻁ ﺍﻟﻣﻭﺟ ﻭﺩ‬
‫ﺩﺍﺧﻝ ﺍﻟﺭﻛﺎﻡ ﻧﺗﻳﺟﺔ ﺗﺟﻣﺩ ﺍﻟﻣﺎء ﺑﺩﺍﺧﻠﻪ ﻭﻋﻣﻝ ﺑﻠﻭﺭﺍﺕ ﻣﻥ ﺍﻟﺟﻠﻳﺩ ﻣﻣﺎ ﻳﺅﺩﻯ ﺍﻟﻰ ﺗﻔﺳﺦ ﺍﻟﺭﻛﺎﻡ ﻭﺗﻬﺷﻣﻪ‪  .‬‬
‫ﺍﻻﻫﻣﻳﻪ ﻭﺍﻻﺳﺗﺧﺩﺍﻡ‪  :‬‬ ‫‪‬‬
‫‪ -‬ﻳﺳﺗﺧﺩﻡ ﻫﺫﺍ ﺍﻻﺧﺗﺑﺎﺭ ﻟﻠﺗﺄﻛﺩ ﻣﻥ ﻣﺗﺎﻧﺔ ﺍﻟﺭﻛﺎﻡ ﻭﻗﺩﺭﺗﻪ ﻋﻠﻰ ﺗﺣﻣ ﻝ ﺍﻟﻌﻭﺍﻣ ﻝ ﺍﻟﺟﻭﻳ ﺔ ﺍﻟﻣﺣﻳﻁ ﺔ ﺑ ﻪ ﺳ ﻭﺍء ﻛ ﺎﻥ ﻣﺳ ﺗﺧﺩﻡ ﻑ‬
‫ﺍﻋﻣﺎﻝ ﺍﻟﻁﺭﻕ ﺍﻭ ﺍﻋﻣﺎﻝ ﺍﻟﺧﺭﺳﺎﻧﺔ‪  .‬‬
‫‪ -‬ﺍﻟﻘﻳﻣﺔ ﺍﻟﻣﺳﻣﻭﺡ ﺑﻬﺎ ﻓﻲ ﺍﻟﻔﻘﺩ ﻧﺗﻳﺟﺔ ﺍﻻﺧﺗﺑﺎﺭ ﺗﺧﺗﻠﻑ ﺑﺎﺧﺗﻼﻑ ﻧﻭﻉ ﺍﻟﺭﻛ ﺎﻡ )ﺧﺷ ﻥ‪-‬ﻧ ﺎﻋﻡ( ﻛﻣ ﺎ ﺍﻧﻬ ﺎ ﺃﻳﺿ ﺎ ﺗﺧﺗﻠ ﻑ ﺑﺗﻐﻳ ﺭ‬
‫ﻧﻭﻉ ﺍﻟﻣﻠﺢ ﺍﻟﻣﺳﺗﺧﺩﻡ ﻟﻼﺧﺗﺑﺎﺭ )ﻛﺑﺭﻳﺗﺎﺕ ﺻﻭﺩﻳﻭﻡ‪-‬ﻛﺑﺭﻳﺗﺎﺕ ﻣﺎﻏﻧﺳﻳﻭﻡ(‪  .‬‬
‫‪ -‬ﻳﻔﺿﻝ ﺍﺳﺗﺧﺩﺍﻡ ﻣﻠﺢ ﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﻣﺎﻏﻧﺳﻳﻭﻡ ﻷﻧﻪ ﻳﻌﻁﻲ ﻧﺗﺎﺋﺞ ﺃﻓﺿﻝ ﻭﺃﺳﺭﻉ‪  .‬‬
‫ﺍﻻﺟﻬﺯﻩ‪  :‬‬ ‫‪‬‬
‫ﻣﻧﺎﺧﻝ ﻗﻳﺎﺳﻳﻪ‪  .‬‬ ‫‪‬‬
‫ﺣﺎﻭﻳﻪ‪  .‬‬ ‫‪‬‬
‫ﺳﻠﻪ ﻣﺣﺎﻁﻪ ﺑﺷﺑﻛﻪ ﻣﻌﺩﻧﻳﻪ‪  .‬‬ ‫‪‬‬
‫‪ ‬ﻣﻧﻅﻡ ﺩﺭﺟﻪ ﺣﺭﺍﺭﻩ‪  .‬‬
‫ﺷﻛﻝ )‪ (١-٧‬ﺳﻠﻪ ‪ ‬‬
‫‪ ‬ﻣﻳﺯﺍﻥ‪  .‬‬
‫‪ ‬ﻓﺭﻥ ﻗﺎﺩﺭ ﻟﻠﺣﻔﺎﻅ ﻋﻠﻲ ﺩﺭﺟﻪ ﺍﻟﺣﺭﺍﺭﻩ ﻋﻧﺩ )‪ (٥ ± ١١٠‬ﺩﺭﺟﻪ ﻣﺋﻭﻳﻪ ‪ ‬‬
‫‪ ‬ﺍﻟﻣﺣﺎﻟﻳﻝ ﺍﻟﻣﺳﺗﺧﺩﻣﻪ ﻓﻲ ﺍﻻﺧﺗﺑﺎﺭ‪  :‬‬
‫ﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﺻﻭﺩﻳﻭﻡ )‪  :(Na2So4‬‬
‫ﻣﺣﻠﻭﻝ ﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﺻﻭﺩﻳﻭﻡ ﺑﺗﺭﻛﻳﺯ ‪ ٢١٥‬ﺟﺭﺍﻡ ﻟﻛﻝ ﻟﺗﺭ ﻓﻲ ﺣﺎﻟﺔ ﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﺻﻭﺩﻳﻭﻡ ﻏﻳﺭ ﺍﻟﻬﻳﺩﺭﺍﺗﻳﺔ ‪  .Na2SO4‬‬
‫ﻣﺣﻠﻭﻝ ﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﺻﻭﺩﻳﻭﻡ ﺑﺗﺭﻛﻳﺯ‪٧٠٠‬ﺟﺭﺍﻡ ﻟﻛﻝ ﻟﺗﺭ ﻓﻲ ﺣﺎﻟﺔ ﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﺻﻭﺩﻳﻭﻡ ﺍﻟﻬﻳﺩﺭﺍﺗﻳﺔ‪.Na2SO4.10H2O.‬‬
‫‪ ‬ﺍﻻﺣﺗﻳﺎﻁﺎﺕ‬
‫‪ ‬ﻳﺟﺏ ﻋﻣﻝ ﺍﻟﻣﺣﻠﻭﻝ ﻋﻧﺩ ﺩﺭﺟﺔ ﺣﺭﺍﺭﺓ )‪ (٣٠-٢٥‬ﺩﺭﺟﻪ ﻣﺋﻭﻳﺔ‪ ،‬ﺑﻌﺩ ﺍﻻﻧﺗﻬﺎء ﻣﻥ ﻋﻣﻝ ﺍﻟﻣﺣﻠ ﻭﻝ ﻳﺟ ﺏ ﺗﻐﻁﻳ ﺔ ﺍﻟﻣﺣﻠ ﻭﻝ‬
‫ﺟﻳﺩﺍ ﻟﻣﻧﻊ ﺍﻟﺗﺑﺧﺭ‪ .‬ﻳﺗﺭﻙ ﺍﻟﻣﺣﻠﻭﻝ ﻝ ﻣﺩﺓ‪ ٤٨‬ﺳﺎﻋﺔ ﻗﺑﻝ ﺍﻟﺑﺩء ﻓﻲ ﺍﺳﺗﺧﺩﺍﻣﻪ‪ .‬ﻋﻧﺩ ﺍﺳﺗﺧﺩﺍﻡ ﺍﻟﻣﺣﻠﻭﻝ ﻓﻲ ﺍﻻﺧﺗﺎﺭ ﻳﺟ ﺏ ﺍﻥ‬
‫ﺗﻛﻭﻥ ﺩﺭﺟﻪ ﺣﺭﺍﺭﺗﻪ )‪ (١±٢١‬ﺩﺭﺟﻪ ﻣﺋﻭﻳﺔ‪  .‬‬
‫ﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﻣﺎﻏﻧﺳﻳﻭﻡ )‪:(MgSo4‬‬
‫ﻳﺗﻡ ﺍﺳﺗﺧﺩﺍﻡ ﻣﺣﻠﻭﻝ ﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﻣﺎﻏﻧﺳﻳﻭﻡ ﺑﺗﺭﻛﻳﺯ ‪ ٣٥٠‬ﺟﺭﺍﻡ ﻟﻛﻝ ﻟﺗﺭ‪  .MgSO4‬‬ ‫‪-‬‬
‫ﻓﻲ ﺣﺎﻟﺔ ﺍﺳﺗﺧﺩﺍﻡ ﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﻣﺎﻏﻧﺳﻳﻭﻡ ﺍﻟﻬﻳﺩﺭﺍﺗﻳﺔ ﻳﺗﻡ ﻋﻣﻝ ﺍﻟﻣﺣﻠﻭﻝ ﺑﺗﺭﻛﻳﺯ ‪ ١٢٣٠‬ﺟﺭﺍﻡ ﻟﻛﻝ ﻟﺗﺭ‬ ‫‪-‬‬
‫)‪  .(MgSO4.7H2O‬‬
‫ﻣﻊ ﻣﺭﺍﻋﺎﺓ ﺍﻻﺣﺗﻳﺎﻁﺎﺕ ﺍﻟﺗﻲ ﺳﺑﻖ ﺷﺭﺣﻬﺎ ﻣﻊ ﻣﺣﻠ ﻭﻝ ﻛﺑﺭﻳﺗ ﺎﺕ ﺍﻟﺻ ﻭﺩﻳﻭﻡ ﺑﺎﻹﺿ ﺎﻓﺔ ﺍﻟ ﻰ ﺍﻥ ﺗﺭﻛﻳ ﺯ ﻣﺣﻠ ﻭﻝ ﻛﺑﺭﻳﺗ ﺎﺕ‬
‫ﺍﻟﻣﺎﻏﻧﺳﻳﻭﻡ ﺍﻟﻬﻳﺩﺭﺍﺗﻳﺔ ﻻ ﻳﺟﺏ ﺍﻥ ﻳﺯﻳﺩ ﻣﻁﻠﻘﺎ ﻋﻥ ‪ ١٤٠٠‬ﺟﺭﺍﻡ ﻟﻛﻝ ﻟﺗﺭ‪.‬‬
‫ﻛﻠﻭﺭﻳﺩ ﺍﻟﺑﺎﺭﻳﻭﻡ )‪:(BaCl2‬‬
‫ﻳﺗﻡ ﻋﻣﻝ ﻣﺣﻠﻭﻝ ﻛﻠﻭﺭﻳﺩ ﺍﻟﺑ ﺎﺭﻳﻭﻡ ﺑﺗﺭﻛﻳ ﺯ ‪ ٥)%٥‬ﺟ ﺭﺍﻡ ﻟﻛ ﻝ ‪١٠٠‬ﺳ ﻡ‪ ٥٠= (٣‬ﺟ ﺭﺍﻡ ﻟﻛ ﻝ ﻟﺗ ﺭ)‪ ،(BaCl2‬ﻳﺳ ﺗﺧﺩﻡ ﻓ ﻲ‬
‫ﻏﺳﻳﻝ ﺍﻟﻌﻳﻧﻪ ﻣﻥ ﻣﺣﺎﻟﻳﻝ ﺍﻟﻛﺑﺭﻳﺗﺎﺕ ﺑﻌﺩ ﺍﻻﺧﺗﺑﺎﺭ‪.‬‬
‫‪ ‬ﺍﻟﻌﻳﻧﺎﺕ‪  :‬‬
‫‪ .i‬ﺍﻟﺭﻛﺎﻡ ﺍﻟﻧﺎﻋﻡ ‪ ‬‬
‫ﺍﻟﺭﻛﺎﻡ ﺍﻟﻧﺎﻋﻡ ﻓﻲ ﻫ ﺫﺍ ﺍﻻﺧﺗﺑ ﺎﺭ ﻳﺟ ﺏ ﺍﻥ ﻳﻣ ﺭ ﻣ ﻥ ﻣﻧﺧ ﻝ‪ ٩٫٥‬ﻣ ﻡ)‪ (٨/٣‬ﺑﻭﺻ ﺔ ﻭﺍﻻ ﺗﻘ ﻝ ﻛﻣﻳ ﺔ ﺍﻟﺭﻛ ﺎﻡ ﺍﻟﻣﺳ ﺗﺧﺩﻣﺔ ﻋ ﻥ‬ ‫‪-‬‬
‫‪ ١٠٠‬ﺟﺭﺍﻡ ﻣﻥ ﺃﺣﺩ ﻫﺫﻩ ﺍﻟﻣﻧﺎﺧﻝ‪.‬‬
‫‪  Passing on:‬‬ ‫‪Retained on‬‬
‫‪9.5mm=(3/8)in‬‬ ‫)‪4.75 mm(#4‬‬
‫)‪  4.75 mm(#4‬‬ ‫)‪2.36 mm(#8‬‬
‫)‪  2.36 mm(#8‬‬ ‫)‪  1.18 mm(#16‬‬
‫)‪  1.18 mm(#16‬‬ ‫)‪600µ(#30‬‬
‫)‪  600µ(#30‬‬ ‫)‪300 µ(#N50‬‬
‫ﺍﻟﺭﻛﺎﻡ ﺍﻟﺧﺷﻥ‪  :‬‬ ‫‪.ii‬‬
‫ﻋﻧﺩ ﺍﺧﺗﺑﺎﺭ ﺍﻟﺭﻛﺎﻡ ﺍﻟﺧﺷﻥ ﻳﺟﺏ ﺍﻥ ﺗﺯﺍﻝ ﻛﻝ ﺍﻟﻣﻭﺍﺩ ﺍﻟﻧﺎﻋﻣﺔ ﻭﺍﻟﺗﻲ ﺗﻣﺭ ﻣﻥ ﻣﻧﺧﻝ ﺭﻗﻡ ‪  .٤‬‬ ‫‪-‬‬
‫ﻳﻣﻛﻥ ﻟﻠﻌﻳﻧﺔ ﺍﻥ ﺗﻛﻭﻥ ﻣﻥ ﺃﺣﺩ ﺍﻟﻣﻧﺎﺧﻝ ﺍﻻﺗﻳﺔ‪  :‬‬ ‫‪-‬‬
‫‪  from‬‬ ‫‪  to‬‬ ‫)‪  Mass(gm‬‬
‫‪  9.5mm=(3/8)in‬‬ ‫)‪  4.75mm(#NO.4‬‬ ‫‪300+‐5‬‬
‫‪  19mm=(3/4)in‬‬ ‫‪  9.5mm(3/8)in‬‬ ‫‪  1000+‐5‬‬
‫‪  12.5mm=(1/2)in‬‬ ‫‪  9.5mm(3/8)in‬‬ ‫‪  330+‐5‬‬
‫‪  19mm=(3/4)in‬‬ ‫‪  12.5mm(1/2)in‬‬ ‫‪  670+‐10‬‬
‫‪  37.5mm=(1.5)in‬‬ ‫‪  19mm=(3/4)in‬‬ ‫‪  1500+‐50‬‬
‫‪  25mm=(1)in‬‬ ‫‪  19mm=(3/4)in‬‬ ‫‪  500+‐30‬‬
‫‪  37.5mm=(1.5)in‬‬ ‫‪25mm=(1)in‬‬ ‫‪1000+‐50‬‬
‫‪  63mm=(2.5)in‬‬ ‫‪  37.5mm =(1.5)in‬‬ ‫‪  5000+‐300‬‬
‫‪  50mm=(2)in‬‬ ‫‪  37.5mm=(1.5)in‬‬ ‫‪  2000+‐200‬‬
‫‪  63mm=(2.5)mm‬‬ ‫‪  50mm=(2)in‬‬ ‫‪  3000+‐300‬‬

‫‪ ‬ﺗﺟﻬﻳﺯ ﻋﻳﻧﻪ ﺍﻻﺧﺗﺑﺎﺭ‪  :‬‬


‫ﻳﺗﻡ ﻏﺳﻝ ﺍﻟﻌﻳﻧﺔ ﻭﺗﺟﻔﻳﻔﻬﺎ ﻓﻲ ﻓﺭﻥ ﺩﺭﺟﺔ ﺣﺭﺍﺭﺗﻪ ‪ ١١٠‬ﺩﺭﺟﺔ ﻣﺋﻭﻳﺔ ﺣﺗﻰ ﺛﺑﺎﺕ ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ‪.‬‬
‫ﻳﺗﻡ ﻓﺻﻝ ﺍﻻﺣﺟﺎﻡ ﺍﻟﻣﺳﺗﺧﺩﻣﺔ ﻑ ﺍﻻﺧﺗﺑﺎﺭ‪.‬‬
‫ﻳ ﺗﻡ ﺍﺧﺗﻳ ﺎﺭ ﺃﺣ ﺩ ﺍﻻﺣﺟ ﺎﻡ ﺍﻟﻣﻭﺟ ﻭﺩﺓ ﻑ ﺍﻟﺟ ﺩﻭﻝ ﺍﻟﺳ ﺎﺑﻖ ﻣ ﻥ ﺍﻟﺭﻛ ﺎﻡ ﺍﻟﺧﺷ ﻥ ﻣ ﺛﻼ ﻭﻭﺯﻥ ﻛ ﻝ ﺣﺟ ﻡ ﻋﻠ ﻰ ﺣ ﺩﻩ ﻛﻣ ﺎ ﻫ ﻭ ﻣﻭﺿ ﺢ‬
‫ﺑﺎﻟﺟﺩﻭﻝ‪.‬‬
‫‪ ‬ﺧﻁﻭﺍﺕ ﺍﻟﺗﺟﺭﺑﻪ‪  :‬‬
‫‪ -١‬ﻳﺗﻡ ﻭﺿﻊ ﻋﻳﻧﺔ ﺍﻟﺭﻛﺎﻡ ﻑ ﺍﻟﻣﺣﻠﻭﻝ )ﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﺻﻭﺩﻳﻭﻡ ﺍﻭ ﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﻣﺎﻏﻧﺳﻳﻭﻡ( ﻭﺍﻟﺫﻱ ﺗﻡ ﺍﻋﺩﺍﺩﻩ ﺳﺎﺑﻘﺎ ﻓﻲ ﺣﺎﻭﻳﺔ‪  .‬‬
‫‪ -٢‬ﻳﺗﻡ ﺗﻐﻁﻳﺔ ﺍﻟﺣﺎﻭﻳﺔ ﺍﻟﺗﻲ ﺗﻡ ﻭﺿﻊ ﺍﻟﺭﻛﺎﻡ ﺑﻬﺎ ﺣﺗﻰ ﻻ ﻳﺣﺩﺙ ﺗﺑﺧﺭ ﻟﻠﻣﺣﻠﻭﻝ‪  .‬‬
‫‪ -٣‬ﺗﺗﺭﻙ ﺍﻟﻌﻳﻧﺔ ﻣﻐﻣﻭﺭﺓ ﻑ ﺍﻟﻣﺣﻠﻭﻝ ﻣﻥ )‪ (١٨-١٦‬ﺳﺎﻋﺔ ﻓﻲ ﺩﺭﺟﺔ ﺣﺭﺍﺭﺓ )‪º (١-+٢١‬ﻣﺋﻭﻳﺔ‪  .‬‬
‫‪ -٤‬ﻳﺗﻡ ﺍﺳﺗﺧﺭﺍﺝ ﺍﻟﻌﻳﻧﺔ ﻣﻥ ﺍﻟﻣﺣﻠﻭﻝ ﻭﺗﺭﻛﻬﺎ ﻓﻲ ﺍﻟﻬﻭﺍء ﻣﻥ )‪ (٢٠-١٠‬ﺩﻗﻳﻘﺔ ﻗﺑﻝ ﻭﺿﻌﻬﺎ ﻓﻔﺭﻥ ﺩﺭﺟﺔ ﺣﺭﺍﺭﺗﻪ‪ ١١٠‬ﺩﺭﺟ ﺔ‬
‫ﻣﺋﻭﻳﺔ ﻟﻣﺩﺓ ‪ ٤‬ﺳﺎﻋﺎﺕ‪  .‬‬
‫‪ -٥‬ﻳﺗﻡ ﺇﻋﺎﺩﺓ ﺍﻟﺧﻁﻭﺍﺕ ﺍﻟﺳﺎﺑﻘﺔ )ﺍﻟﺩﻭﺭﺓ ﺍﻟﻭﺍﺣﺩﺓ( ‪ ٥‬ﻣﺭﺍﺕ‪  .‬‬
‫‪ -٦‬ﻳﺗﻡ ﺍﺳﺗﺧﺭﺍﺝ ﺍﻟﺭﻛﺎﻡ ﻣﻥ ﺍﻟﺣﺎﻭﻳﺔ ﺍﻟﻣﻭﺟﻭﺩ ﺑﻬﺎ ﻣﻠﺢ ﺍﻟﻛﺑﺭﻳﺗﺎﺕ ﻭﻭﺿ ﻌﻪ ﻓ ﻲ ﺣﺎﻭﻳ ﺔ ﺃﺧ ﺭﻯ ﻭﻳ ﺗﻡ ﻏﺳ ﻠﻪ ﺑﻣﺣﻠ ﻭﻝ ﻛﻠﻭﺭﻳ ﺩ‬
‫ﺍﻟﺑﺎﺭﻳﻭﻡ ﻟﻠﺗﺧﻠﺹ ﻣﻥ ﺍﻟﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﻣﻭﺟﻭﺩﺓ ﺑﺎﻟﺭﻛﺎﻡ‪  .‬‬
‫‪ -٧‬ﺑﻌﺩ ﺇﺯﺍﻟﺔ ﻛﺑﺭﻳﺗﺎﺕ ﺍﻟﺻﻭﺩﻳﻭﻡ ﺍﻭ ﺍﻟﻣﺎﻏﻧﺳﻳﻭﻡ ﻣﻥ ﺍﻟﺭﻛﺎﻡ ﻳﺗﻡ ﺗﺟﻔﻳﻑ ﺍﻟﻌﻳﻧﺔ ﻓﻲ ﻓﺭﻥ ﺩﺭﺟﺔ ﺣﺭﺍﺭﺗﻪ ‪ ١١٠‬ﺩﺭﺟﺔ ﻣﺋﻭﻳﺔ‪  .‬‬
‫‪ -٨‬ﻳﺗﻡ ﺍﺳﺗﺧﺩﺍﻡ ﻣﻧﺧﻝ ﺃﺻﻐﺭ ﻣﻥ ﺍﻟﻣﻧﺎﺧﻝ ﺍﻟﻣﺳﺗﺧﺩﻣﺔ ﻓﻲ ﺍﻻﺧﺗﺑﺎﺭ‪  .‬‬
‫‪  from‬‬ ‫‪  to‬‬ ‫‪use‬‬
‫‪37.5mm‬‬ ‫‪19mm‬‬ ‫‪  16 mm‬‬
‫‪  19mm‬‬ ‫‪9.5mm‬‬ ‫‪8mm‬‬
‫‪  9.5mm‬‬ ‫)‪  4.75 mm (#4‬‬ ‫‪2.36mm‬‬
‫‪ -٩‬ﻳﺗﻡ ﻭﺯﻥ ﻛﻝ ﻣﻧﺧﻝ ﻋﻠﻰ ﺣﺩﻩ ﻭﺗﻌﻳﻳﻥ ﻧﺳﺑﺔ ﺍﻟﻔﻘﺩ ﻑ ﻛ ﻝ ﻣﻧﺧ ﻝ )ﺑﺣﻳ ﺙ ﺗﻛ ﻭﻥ ﺍﻟﻣ ﻭﺍﺩ ﺍﻻﻧﻌ ﻡ ﻣ ﻥ ﺍﻟﻣﻧﺧ ﻝ ﺍﻟﻣﺳ ﺗﺧﺩﻡ ﺑﻌ ﺩ‬
‫ﺍﻻﺧﺗﺑﺎﺭ ﻳﻌﺑﺭ ﻋﻧﻬﺎ ﺑﻧﺳﺑﺔ ﻣﻥ ﺍﻟﻔﻘﺩ ﺍﻟﻛﻠﻲ(‪  .‬‬
‫‪ -١٠‬ﻳﺗﻡ ﺣﺳﺎﺏ ﺍﻟﻔﻘﺩ ﻣﻥ ﺍﻟﻭﺯﻥ ﻟﻛﻝ ﻣﻧﺧﻝ ﺛﻡ ﺣﺳﺎﺏ ﺍﻟﻣﺗﻭﺳﻁ ﻭﺣﺳﺎﺏ ﻧﺳﺑﺔ ﺍﻟﻔﻘﺩ ﺍﻟﻛﻠﻳﺔ‪  .‬‬
‫‪ -١١‬ﺗﻛ ﻭﻥ ﻧﺳ ﺑﺔ ﺍﻟﻔﻘ ﺩ ﻓ ﻲ ﺍﻟﺭﻛ ﺎﻡ ﻧﺗﻳﺟ ﺔ ﻛﺑﺭﻳﺗ ﺎﺕ ﺍﻟﺻ ﻭﺩﻳﻭﻡ)‪% (٢٠-٩) ،% (١٦-٦‬ﻓ ﻲ ﺣﺎﻟ ﺔ ﺍﺳ ﺗﺧﺩﺍﻡ ﻛﺑﺭﻳﺗ ﺎﺕ‬
‫ﺍﻟﻣﺎﻏﻧﺳﻳﻭﻡ‪  .‬‬
‫‪ ‬‬

‫ﺷﻛﻝ )‪ (٢-٧‬ﻳﻭﺿﺢ ﺗﺎﺛﻳﺭ ﻣﺣﻠﻭﻝ ﺍﻟﻛﺑﺭﻳﺗﺎﺕ ﻋﻠﻲ ﻋﻳﻧﻪ ﺍﻟﺭﻛﺎﻡ ‪ ‬‬


‫ﺗﺟﺭﺑﺔ ﺭﻗﻡ ‪-٨-‬‬
‫ﺍﺧﺗﺑﺎﺭ ﺍﻻﺧﺗﺭﺍﻕ ﻟﻸﺳﻔﻠﺕ‬
‫‪  Penetration test of Asphalt cement‬‬
‫‪  ASTM D5‬‬
‫‪ ‬ﺍﻟﻐﺭﺽ ‪:‬‬
‫ﻟﺣﺳﺎﺏ ﻗﻳﻣﺔ ﺍﻻﺧﺗﺭﺍﻕ ﻟﻠﻣﻭﺍﺩ ﺍﻻﺳﻔﻠﺗﻳﺔ ﺍﻟﺻﻠﺑﺔ ﻭﺍﻟﺷﺑﻪ ﺻﻠﺑﺔ‪.‬‬
‫‪ ‬ﺍﻻﻫﻣﻳﺔ ﻭﺍﻻﺳﺗﺧﺩﺍﻡ ‪:‬‬
‫ﺍﺧﺗﺑﺎﺭ ﺍﻻﺧﺗﺭﺍﻕ ﻳﺳﺗﺧﺩﻡ ﻟﻘﻳﺎﺱ ﺍﻟﻠﺯﻭﺟﺔ‪ ،‬ﺗﺷﻳﺭ ﻗﻳﻣﺔ ﺍﻻﺧﺗﺭﺍﻕ ﺍﻟﻌﺎﻟﻳﺔ ﺍﻟﻲ ﻟﺯﻭﺟﺔ ﺍﻗﻝ )ﺻﻼﺑﺔ ﺍﻗﻝ(‪.‬‬
‫‪ ‬ﺍﻻﺟﻬﺯﺓ‪:‬‬
‫ﺟﻬﺎﺯ ﺍﻻﺧﺗﺭﺍﻕ ﻭﺍﺑﺭﺓ ﻣﻌﺩﻧﻳﺔ‪،‬ﺷﻛﻝ )‪(١-٨‬‬
‫ﻭﻋﺎء‪ ،‬ﺣﻣﺎﻡ ﻣﺎﺋﻲ‪ ،Transfer Dish ،‬ﺳﺎﻋﻪ ﺍﻳﻘﺎﻑ ﻭ ﺗﺭﻣﻭﻣﺗﺭ‪.‬‬
‫‪ ‬ﺧﻁﻭﺍﺕ ﺍﻟﺗﺟﺭﺑﺔ ‪:‬‬
‫‪ .١‬ﺗﺳﺧﻳﻥ ﻋﻳﻧﺔ ﺍﻻﺳﻔﻠﺕ ﻟﻠﺣﺎﻟﺔ ﺍﻟﺳﺎﺋﻠﺔ ﺣﺗﻲ ﻳﺳﻬﻝ ﺻﺑﻬﺎ‪.‬‬
‫‪ .٢‬ﺻﺏ ﺍﻟﻌﻳﻧﺔ ﻓﻲ ﺍﻟﻭﻋﺎء‪ ،‬ﺗﺟﻧﺏ ﺗﻛﻭﻥ ﺍﻟﻔﻘﺎﻋﺎﺕ ﻓﻲ ﺍﻟﻌﻳﻧﺔ ﻭﺗﺭﻛﻬﺎ ﻟﺗﺑﺭﺩ ﻟﻣ ﺩﺓ‬
‫‪ ١‬ﺳﺎﻋﺔ ﻋﻠﻲ ﺍﻻﻗﻝ‪  .‬‬
‫‪ .٣‬ﻭﺿ ﻊ ﺍﻟﻌﻳﻧ ﺔ ﻭﺍﻝ ‪ Transfer  Dish‬ﻓ ﻲ ﺍﻟﺣﻣ ﺎﻡ ﺍﻟﻣ ﺎﺋﻲ ﻋﻧ ﺩ ﺩﺭﺟ ﺔ ﺣ ﺭﺍﺭﺓ‬
‫‪ ٢٥‬ﺩﺭﺟﺔ ﻣﺋﻭﻳﺔ ﻟﻣﺩﺓ ﺗﺗﺭﺍﻭﺡ ﺑﻳﻥ )‪ (٢ – ١‬ﺳﺎﻋﺔ‪.‬‬
‫‪ .٤‬ﺗﻧﻅﻳ ﻑ ﺍﻻﺑ ﺭﺓ ﻭﺗﺟﻔﻳﻔﻬ ﺎ )ﺑﺎﺳ ﺗﺧﺩﺍﻡ ﻣ ﺫﻳﺏ ﻭﻗﻁﻌ ﻪ ﻗﻣ ﺎﺵ ﻧﻅﻳﻔ ﺔ(‪ ،‬ﻭﻭﺿ ﻊ‬
‫ﺍﻻﺑ ﺭﺓ ﻓ ﻲ ﺟﻬ ﺎﺯ ﺍﻻﺧﺗ ﺭﺍﻕ ﻭﺍﺿ ﺎﻓﺔ ﻛﺗﻠ ﻪ )‪ ٥٠‬ﺟ ﻡ( ﻓ ﻭﻕ ﺍﻻﺑ ﺭﺓ‪ ،‬ﻟﺟﻌ ﻝ‬
‫ﺍﻟﺣﻣﻝ ﺍﻟﻣﺗﺣﺭﻙ ﺍﻟﻛﻠﻲ ‪ ١٠٠‬ﺟﻡ‪  .‬‬
‫‪ .٥‬ﻭﺿ ﻊ ﺍﻟﻭﻋ ﺎء ﻓ ﻲ ﺍﻝ ‪ ،Transfer  Dish‬ﺑﺣﻳ ﺙ ﺗﻛ ﻭﻥ ﺍﻟﻌﻳﻧ ﺔ ﻣﻐﻁ ﺎﺓ ﺗﻣﺎﻣ ﺎ‬
‫ﺑﺎﻟﻣﻳﺎﻩ ﻣﻥ ﺍﻟﺣﻣﺎﻡ ﺍﻟﻣﺎﺋﻲ‪ .‬ﺍﻟﺗﺄﻛﺩ ﻣﻥ ﺍﺳﺗﻭﺍء ﺍﻟﺟﻬﺎﺯ ﺑﻭﺍﺳﻁﺔ ﻣﺅﺷﺭ ﺍﻟﺗﺳﻭﻳﺔ‪  .‬‬
‫‪ .٦‬ﺇﻧﺯﺍﻝ ﺍﻻﺑﺭﺓ ﺑﺑﻁء ﺣﺗﻲ ﺗﻠﻣﺱ ﻣﻘﺩﻣﺔ ﺍﻻﺑﺭﺓ ﺳﻁﺢ ﺍﻟﻌﻳﻧﺔ‪  .‬‬
‫‪ .٧‬ﺟﻌ ﻝ ﺍﻻﺑ ﺭﺓ ﺗﺳ ﻘﻁ ﺳ ﻘﻭﻁ‬
‫ﺷﻛﻝ )‪ (١-٨‬ﺍﻻﺟﻬﺯﺓ ﺍﻟﻣﺳﺗﺧﺩﻣﺔ ﻓﻲ ﺍﺧﺗﺑﺎﺭ ﺍﻻﺧﺗﺭﺍﻕ ‪ ٥  ‬ﺛ ﻭﺍﻧﻲ‪ ،‬ﺿ ﺑﻁ ﺍﻟﺟﻬ ﺎﺯ‬ ‫ﺣﺭ ﺗﺣ ﺕ ﺗ ﺄﺛﻳﺭ ﻭﺯﻧﻬ ﺎ ﻟﻣ ﺩﺓ‬
‫ﻷﻗ ﺭﺏ ‪ ٠٬١‬ﻣ ﻡ‪ ،‬ﺷ ﻛﻝ )‪-٨‬‬ ‫ﻟﻘﻳﺎﺱ ﻣﺳﺎﻓﺔ ﺍﺧﺗ ﺭﺍﻕ ﺍﻻﺑ ﺭﺓ‬
‫‪  .(٢‬‬
‫‪ .٨‬ﺍﺧﺫ ‪ ٣‬ﻗﺭﺍءﺍﺕ ﻻﺧﺗﺭﺍﻕ ﺍﻻﺑﺭﺓ ﻟﻠﻌﻳﻧﺔ ﻋﻠﻲ ﻣﺳﺎﻓﺎﺕ ﻻ ﺗﻘﻝ ﻋﻥ ‪ ١٠‬ﻣﻡ ﻣﻥ ﺟﺩﺍﺭ ﺍﻟﻭﻋﺎء ﻭﺍﻟﻣﺳﺎﻓﺔ ﺑﻳﻥ ﺍﻟﻘﺭﺍءﺍﺕ ﻻ ﺗﻘﻝ‬
‫ﻋﻥ ‪ ١٠‬ﻣﻡ‪  .‬‬
‫‪ ‬ﺍﻟﺗﻘﺭﻳﺭ ‪  :‬‬
‫ﻣﺗﻭﺳﻁ ﺍﻟﻘﺭﺍﺭﺍﺕ ﻷﻗﺭﺏ ﺭﻗﻡ ﺻﺣﻳﺢ‪.‬‬

‫ﺷﻛﻝ )‪ (٢-٨‬ﻗﻳﻣﻪ ﺍﻻﺧﺗﺭﺍﻕ‬


Penetration Test of Asphalt Cement
Penetration Values:

1stPenetration Value  A =   mm 


2nd Penetration Value  B =    mm 
3rd Penetration Value  C =    mm 
Average    (A+B+C)/3   
      mm 

 
‫ﺗﺟﺭﺑﻪ ﺭﻗﻡ ‪-٩-‬‬
‫‪ ‬ﻗﻳﺎﺱ ﻟﺯﻭﺟﺔ ﺍﻻﺳﻔﻠﺕ ﺑﺎﺳﺗﺧﺩﺍﻡ ﻣﻘﻳﺎﺱ ﺍﻟﻠﺯﻭﺟﺔ ﺍﻟﺩﻭﺍﺭ‬
‫‪Viscosity of Asphalt Cement by Rotational Viscometer ‬‬
‫‪ASTM D4402‬‬

‫‪ ‬ﺍﻟﻐﺭﺽ ‪  :‬‬ ‫‪‬‬


‫ﻟﺗﻌﻳﻥ ﻟﺯﻭﺟﺔ ﺍﻷﺳﻔﻠﺕ ﺍﻟﻅﺎﻫﺭﻳﺔ ﻋﻧﺩ ﺩﺭﺟﻪ ﺣﺭﺍﺭﻩ )‪ (٣٨:٢٦٠‬ﺩﺭﺟ ﻪ ﻣﺋﻭﻳ ﻪ ﺑﺈﺳ ﺗﺧﺩﺍﻡ ﻣﻘﻳ ﺎﺱ ﺍﻟﻠﺯﻭﺟ ﺔ ﺍﻟ ﺩﻭﺍﺭ ﻭﺗﺿ ﺑﻁ ﺩﺭﺟ ﻪ‬
‫ﺣﺭﺍﺭﻩ ﺍﻻﺧﺗﺑﺎﺭ ﺑﻭﺍﺳﻁﺔ ﻏﺭﻓﺔ ﺍﻟﺗﺣﻛﻡ ﺍﻟﺣﺭﺍﺭﻳﺔ‪.‬‬
‫‪ ‬ﺍﻻﻫﻣﻳﺔ ﻭﺍﻻﺳﺗﺧﺩﺍﻡ ‪:‬‬
‫ﺍﻟﺗﺄﻛﺩ ﻣﻥ ﻟﺯﻭﺟﺔ ﺍﻻﺳﻔﻠﺕ ﻗﺑﻝ ﻧﻘﻠﻪ‪ ،‬ﺿﺧﻪ ﻓﻲ ﺍﻟﻣﻭﺍﺳﻳﺭ ﻭ ﻻﺧﺗﺑﺎﺭﺍﺕ ﺿﺑﻁ ﺍﻟﺟﻭﺩﺓ‪ .‬ﻳﺳﺗﺧﺩﻡ ﻟﺗﻌﻳﻳﻥ ﺩﺭﺟﺔ ﺣﺭﺍﺭﺓ ﺍﻟﺧﻠﻁ‬
‫ﻭﺍﻟﺩﻣﻙ ﻟﻠﺧﻠﻁﺔ ﺍﻻﺳﻔﻠﺗﻳﺔ‪.‬ﻫﺫﺍ ﺍﻻﺧﺗﺑﺎﺭ ﻳﺳﺗﺧﺩﻡ ﻓﻲ ﺗﺩﺭﺝ ﺍﻻﺳﻔﻠﺕ ﻓﻲ ﻧﻅﺎﻡ ﺍﻟﺳﻭﺑﺭ ﺑﻳﻑ )‪  .(superpave‬‬
‫‪ ‬ﺍﻻﺟﻬﺯﺓ‪:‬‬
‫ﻣﻘﻳﺎﺱ ﺍﻟﻠﺯﻭﺟﺔ ﺍﻟﺩﻭﺍﺭ‬
‫ﺍﺑﺭﺓ ﻗﻳﺎﺳﻳﺔ‬
‫ﺍﺩﺍﻩ ﺍﺳﺗﺧﺭﺍﺝ )‪(Extracting Tool‬‬
‫ﻧﻅﺎﻡ ﺣﺭﺍﺭﻱ ﻳﺗﻛﻭﻥ ﻣﻥ ﺣﺎﻭﻳﺔ ﺣﺭﺍﺭﻳﺔ‪ ،‬ﺍﻧﺑﻭﺑﻪ ﻣﻌﺩﻧﻳﻪ ﻟﻠﻌﻳﻧﻪ‪ ،‬ﻣﻧﻅﻡ ﺣﺭﺍﺭﺓ ﻭﺟﻬﺎﺯ ﻟﺭﺳﻡ ﺍﻟﻌﻼﻗﻪ ﺑﻳﻥ ﺍﻟﻠﺯﻭﺟﻪ ﻭﺩﺭﺟﻪ ﺍﻟﺣﺭﺍﺭﺓ‪.‬‬

‫‪ ‬ﺧﻁﻭﺍﺕ ﺍﻟﺗﺟﺭﺑﺔ ‪:‬‬


‫‪ .١‬ﺗﺷﻐﻳﻝ ﺟﻬ ﺎﺯ ﺍﻻﺧﺗﺑ ﺎﺭ ﻭﺿ ﺑﻁ ﺩﺭﺟ ﻪ ﺣ ﺭﺍﺭﻩ ﺍﻻﺧﺗﺑ ﺎﺭ ﻣ ﻥ ﺧ ﻼﻝ‬
‫ﻣﻧﻅﻡ ﺍﻟﺣﺭﺍﺭﺓ‪  .‬‬
‫‪ .٢‬ﺍﻻﻧﺗﻅ ﺎﺭ )‪ (١ :٠٫٥‬ﺳ ﺎﻋﻪ ﺍﻭ ﻋﻧ ﺩ ﺍﻟﻭﺻ ﻭﻝ ﻟﺩﺭﺟ ﻪ ﺍﻟﺣ ﺭﺍﺭﻩ‬
‫ﺍﻟﻣﻁﻠﻭﺑﻪ )ﻓﺣﺹ ﻟﻣﺑﻪ ﺍﻟﻣﻧﻅﻡ(‪  .‬‬
‫‪٣‬‬
‫‪ .٣‬ﻳﺗﻡ ﺍﺿﺎﻓﻪ ﻋﻳﻧﻪ ﺍﻟﺑﺗ ﻭﻣﻳﻥ ﻓ ﻲ ﺍﻟﻭﻋ ﺎء ﺣ ﻭﺍﻟﻲ )‪ (٨:١٠‬ﺳ ﻡ ﺑﺣﻳ ﺙ‬
‫ﻳﻛ ﻭﻥ ﻣﺳ ﺗﻭﻱ ﺍﻟﺑﺗ ﻭﻣﻳﻥ ﺍﻋﻠ ﻲ ﻣ ﻥ ﺍﻟﺟ ﺯء ﺍﻟﻣﺧﺭﻭﻁ ﻲ ﻟﻺﺑ ﺭﻩ‬
‫ﺑﺣﻭﺍﻟﻲ )‪ (٣‬ﻣﻡ‪  .‬‬
‫‪ .٤‬ﺑﺈﺳ ﺗﺧﺩﺍﻡ ﺍﺩﺍﻩ ﺍﻻﺳ ﺗﺧﺭﺍﺝ )‪ ،(Extracting  tool‬ﻭﺿ ﻊ ﺍﻧﺑﻭﺑ ﻪ‬
‫ﺍﻻﺧﺗﺑﺎﺭ ﻓﻲ ﺍﻟﻭﻋﺎء ﺍﻟﺣﺭﺍﺭﻱ‪  .‬‬
‫‪ .٥‬ﻳﺗﻡ ﺍﺧﺗﻳﺎﺭ ﺍﻻﺑﺭﻩ ﺍﻟﻣﻧﺎﺳﺑﻪ ﻭﻭﺿ ﻌﻬﺎ ﻓ ﻲ ﺍﻧﺑﻭﺑ ﻪ ﺍﻻﺧﺗﺑ ﺎﺭ‪ .‬ﻛ ﻼ ﻣ ﻥ‬
‫ﺍﻻﺑ ﺭﻩ ﺭﻗ ﻡ ‪ ٢٧‬ﻭ ﺍﻻﺑ ﺭﻩ ﺭﻗ ﻡ ‪ ٢٠‬ﺗﺳ ﺗﺧﺩﻡ ﻓ ﻲ ﺗﻌﻳ ﻳﻥ ﻟﺯﻭﺟ ﻪ‬
‫ﺍﻻﺳﻔﻠﺕ‪  .‬‬
‫‪ .٦‬ﺍﻻﻧﺗﻅ ﺎﺭ ﻟﻭﺻ ﻭﻝ ﺍﻻﺳ ﻔﻠﺕ ﻟﺩﺭﺟ ﻪ ﺣ ﺭﺍﺭﻩ ﺍﻻﺧﺗﺑ ﺎﺭ ﺟ ﻭﺍﻟﻲ ‪١٥‬‬
‫ﺩﻗﻳﻘﻪ‪  .‬‬
‫‪ .٧‬ﺗﺷﻐﻳﻝ ﺍﻟﺟﻬﺎﺯ )‪ (Viscometer‬ﺑﻣﻌﺩﻝ ‪ ٢٠‬ﻟﻔﻪ‪/‬ﺩﻗﻳﻘﻪ‪  .‬‬
‫‪ .٨‬ﺗﺳﺟﻳﻝ ‪ ٣‬ﻗﺭﺍءﺍﺕ ﺧﻼﻝ ‪ ٦٠‬ﺛﺎﻧﻳﻪ ﻋﻧﺩ ﻛﻝ ﺩﺭﺟﻪ ﺣﺭﺍﺭﻩ ﻟﻼﺧﺗﺑﺎﺭ‪  .‬‬
‫‪ .٩‬ﺿ ﺭﺏ ﻣﻌﺎﻣ ﻝ ﺍﻟﻠﺯﻭﺟ ﻪ ﻭﻗ ﺭﺍءﻩ ﺟﻬ ﺎﺯ ﺍﻟﻠﺯﻭﺟ ﻪ ﺍﻟ ﺩﻭﺍﺭ ﻟﻠﺣﺻ ﻭﻝ‬
‫)‪.(CP‬‬ ‫ﺷﻛﻝ )‪ (١-٩‬ﺟﻬﺎﺯ ﺍﻟﻠﺯﻭﺟﻪ ﺍﻟﺩﻭﺍﺭ‬ ‫ﻋﻠ ﻲ ﺍﻟﻠﺯﻭﺟ ﻪ ﺑﻭﺣ ﺩﻩ‬
‫‪ ‬ﺍﻟﺗﻘﺭﻳﺭ ‪  :‬‬
‫ﻣﺗﻭﺳﻁ ﺍﻟﻠﺯﻭﺟﻪ ﻋﻧﺩ ﻛﻝ ﺩﺭﺟﻪ ﺣﺭﺍﺭﻩ‪.‬‬
‫ﺭﻗﻡ ﺍﻻﺑﺭﻩ ﺍﻟﻣﺳﺗﺧﺩﻣﻪ ﻭﺳﺭﻋﻪ ﺍﻟﺩﻭﺭﺍﻥ‪.‬‬
Viscosity of Asphalt Cement by Rotational Viscometer 
 

Spindle # 
Rotational Speed 
Temp. (R)   
Viscosity (CP)     

 
‫( ﺍﻟﻌﻼﻗﻪ ﺑﻴﻦ ﺩﺭﺟﻪ ﺍﻟﺤﺮﺍﺭﻩ ﻭﺍﻟﻠﺰﻭﺟﻪ‬٢-٩) ‫ﺷﻜﻞ‬

For Mixing:  For Compaction:
Viscosity  Temp. Viscosity Temp. 
(CP)  (R)  (CP)  (R) 
150  250  
190  310  
‫ﺗﺟﺭﺑﻪ ﺭﻗﻡ ‪-١٠-‬‬
‫ﺧﺻﺎﺋﺹ ﺍﻟﺗﺭﺑﻪ ﺍﻟﻣﺩﻣﻭﻛﻪ ﺑﺎﺳﺗﺧﺩﺍﻡ ﺍﻟﺑﺭﻭﻛﺗﻭﺭ ﺍﻟﻣﻌﺩﻝ‬
‫‪Laboratory Compaction Characteristics of Soil Using Modified Effort‬‬
‫‪  ASTM D1557‬‬
‫‪ ‬ﺍﻟﻐﺭﺽ‪:‬‬
‫ﻳﻐﻁﻲ ﻫﺫﺍ ﺍﻻﺧﺗﺑﺎﺭ ﻁﺭﻕ ﺍﻟﺩﻣﻙ ﺍﻟﻣﻌﻣﻠﻳﻪ ﺍﻟﻣﺳﺗﺧﺩﻣﻪ ﻓﻲ ﺗﻌﻳﻳﻥ ﺍﻟﻌﻼﻗﻪ ﺑ ﻳﻥ ﺍﻟﻣﺣﺗ ﻭﻱ ﺍﻟﺭﻁ ﻭﺑﻲ ﻭﺍﻟﻛﺛﺎﻓ ﻪ ﺍﻟﺟﺎﻓ ﻪ ﻟﻠﺗﺭﺑ ﻪ )ﻣﻧﺣﻧ ﻲ‬
‫ﺍﻟﺩﻣﻙ(‪ ،‬ﺗﺩﻣﻙ ﺍﻟﻌﻳﻧﺎﺕ ﻓﻲ ﻗﺎﻟﺏ ﻗﻳﺎﺳﻲ ﺑﻘﻁﺭ ‪ ٤‬ﺍﻭ ‪ ٦‬ﺑﻭﺻﻪ ﺑﻭﺍﺳﻁﻪ ﻣﻁﺭﻗﻪ ﺗﺯﻥ ‪ ١٠‬ﺭﻁﻝ ﺗﺳﻘﻁ ﺳﻘﻭﻁ ﺣﺭ ﺗﺣﺕ ﺗﺎﺛﻳﺭ ﻭﺯﻧﻬﺎ‬
‫ﻣﻥ ﺍﺭﺗﻔﺎﻉ ‪ ١٨‬ﺑﻭﺻﻪ‪.‬‬
‫ﻳﺳﻣﺢ ﺑﺎﺟﺭﺍء ﻫﺫﺍ ﺍﻻﺧﺗﺑﺎﺭ ﻋﻠﻲ ﺍﻟﻣﻭﺍﺩ ﺍﻟﻣﺣﺗﻭﺍﻩ ﻋﻠﻲ ‪ %٣٠‬ﺍﻭ ﺍﻗﻝ ﻣﻥ ﻭﺯﻧﻬﺎ ﻣﺣﺟﻭﺯﻩ ﻋﻠﻲ ﺍﻟﻣﻧﺧﻝ )‪ (٣/٤‬ﺑﻭﺻﻪ‪.‬‬
‫ﻁﺭﻳﻘﻪ )ﺝ(‬ ‫ﻁﺭﻳﻘﻪ )ﺏ(‬ ‫ﻁﺭﻳﻘﻪ )ﺃ(‬
‫ﻗﻁﺭ ‪ ٦‬ﺑﻭﺻﻪ‬ ‫ﻗﻁﺭ ‪ ٤‬ﺑﻭﺻﻪ‬ ‫ﻗﻁﺭ ‪ ٤‬ﺑﻭﺻﻪ‬ ‫ﺍﻟﻘﺎﻟﺏ ﺍﻟﻣﺳﺗﺧﺩﻡ‬
‫ﺍﻟﻣ ﺎﺭ ﻣ ﻥ ﺍﻟﻣﻧﺧ ﻝ ‪ ٣/٤‬ﺑﻭﺻ ﻪ‪ .‬ﻓ ﻲ‬ ‫ﺍﻟﻣﺎﺭ ﻣﻥ ﺍﻟﻣﻧﺧﻝ ‪ ٣/٨‬ﺑﻭﺻ ﻪ‪ .‬ﻓ ﻲ ﺣﺎﻟ ﻪ‬ ‫ﺍﻟﻣ ﺎﺭ ﻣ ﻥ ﺍﻟﻣﻧﺧ ﻝ ﺭﻗ ﻡ ‪٤‬‬ ‫ﺍﻟﻣﻭﺍﺩ ﺍﻟﻣﺳﺗﺧﺩﻣﻪ‬
‫ﺣﺎﻟ ﻪ ﺯﻳ ﺎﺩﻩ ﻧﺳ ﺑﻪ ﺍﻟﻣ ﻭﺍﺩ ﺍﻟﻣﺣﺟ ﻭﺯﻩ‬ ‫ﺯﻳ ﺎﺩﻩ ﻧﺳ ﺑﻪ ﺍﻟﻣ ﻭﺍﺩ ﺍﻟﻣﺣﺟ ﻭﺯﻩ ﻋﻠ ﻲ‬ ‫ﺑﺣﻳﺙ ﻳﻛ ﻭﻥ ﺍﻟﻣﺣﺟ ﻭﺯ ﻋﻠ ﻲ‬
‫ﻋﻠ ﻲ ﺍﻟﻣﻧﺧ ﻝ ‪ ٣/٨‬ﺑﻭﺻ ﻪ ﺍﻛﺑ ﺭ ﻣ ﻥ‬ ‫ﺍﻟﻣﻧﺧ ﻝ ﺭﻗ ﻡ ‪ ٤‬ﻋ ﻥ ‪ %٢٠‬ﻭﺍﻟﻣﺣﺟ ﻭﺯ‬ ‫ﺍﻟﻣﻧﺧ ﻝ ﺭﻗ ﻡ ‪ ٤‬ﺍﻗ ﻝ ﻣ ﻥ ﺍﻭ‬
‫‪ %٢٠‬ﻭﺍﻟﻣﺣﺟ ﻭﺯ ﻋﻠ ﻲ ﺍﻟﻣﻧﺧ ﻝ ‪٣/٤‬‬ ‫ﻋﻠ ﻲ ﺍﻟﻣﻧﺧ ﻝ ‪ ٣/٨‬ﺑﻭﺻ ﻪ ﺍﻗ ﻝ ﻣ ﻥ‬ ‫ﻳﺳ ﺎﻭﻱ ‪ %٢٠‬ﻣ ﻥ ﻭﺯﻥ‬
‫ﺑﻭﺻﻪ ﺍﻗﻝ ﻣﻥ ‪%٣٠‬‬ ‫‪.%٢٠‬‬ ‫ﺍﻟﻌﻳﻧﻪ‪.‬‬
‫‪ ٥‬ﻁﺑﻘﺎﺕ‬ ‫‪ ٥‬ﻁﺑﻘﺎﺕ‬ ‫‪ ٥‬ﻁﺑﻘﺎﺕ‬ ‫ﻋﺩﺩ ﺍﻟﻁﺑﻘﺎﺕ‬
‫‪ ٥٦‬ﺩﻗﻪ‪/‬ﻁﺑﻘﻪ‬ ‫‪ ٢٥‬ﺩﻗﻪ‪/‬ﻁﺑﻘﻪ‬ ‫‪ ٢٥‬ﺩﻗﻪ‪/‬ﻁﺑﻘﻪ‬ ‫ﻋﺩﺩ ﺍﻟﺩﻗﺎﺕ‬

‫‪ ‬ﺍﻻﻫﻣﻳﻪ ﻭﺍﻻﺳﺗﺧﺩﺍﻡ‪:‬‬
‫ﺗﺩﻣﻙ ﻁﺑﻘﺎﺕ ﺍﻟﺭﺻﻑ )ﻁﺑﻘﻪ ﺍﻻﺳﺎﺱ‪ ،‬ﺍﻻﺳﺎﺱ ﺍﻟﻣﺳﺎﻋﺩ‪ ،‬ﻭﻁﺑﻘﻪ ﺍﻟﺗﺎﺳ ﻳﺱ( ﻟﻠﻭﺻ ﻭﻝ ﻻﻗﺻ ﻲ ﻛﺛﺎﻓ ﻪ ﻟﻠﺣﺻ ﻭﻝ ﻋﻠ ﻲ ﺍﻟﺧﺻ ﺎﺋﺹ‬
‫ﺍﻟﻬﻧﺩﺳﻳﻪ ﺍﻟﻣﻁﻠﻭﺑﻪ ﻣﻥ ﺣﻳﺙ )ﻣﻘﺎﻭﻣﻪ ﺍﻟﻘﺹ‪ ،‬ﻗﺎﺑﻠﻳﻪ ﺍﻧﺿﻐﺎﻁ ﺍﻟﺗﺭﺑﻪ ﺍﻭ ﻧﻔﺎﺫﻳﻪ ﺍﻟﺗﺭﺑﻪ(‪.‬‬
‫ﺣﺳﺎﺏ ﻧﺳﺑﻪ ﺍﻟﺩﻣﻙ ﻭﻣﺣﺗﻭﻱ ﺍﻟﺭﻁﻭﺑﻪ ﺍﻟﻼﺯﻡ ﻟﺗﺣﻘﻳﻖ ﺍﻟﺧﺻﺎﺋﺹ ﺍﻟﻣﻁﻠﻭﺑﻪ‪.‬‬
‫‪ ‬ﺍﻻﺟﻬﺯﻩ‪  :‬‬
‫‪ ‬ﻗﺎﻟ ﺏ ﻗﻳﺎﺳ ﻲ ﺑﻘﻁ ﺭ ‪ ٤‬ﺑﻭﺻ ﻪ ﻭﺍﺭﺗﻔ ﺎﻉ ‪ ٤٫٦‬ﺑﻭﺻ ﻪ ﻟﻠﺗﺭﺑ ﻪ ﺍﻟﻧﺎﻋﻣ ﻪ‬
‫)ﻁﺭﻳﻘ ﻪ )ﺃ(‪) ،‬ﺏ(( ﻭﺑﻘﻁ ﺭ ‪ ٦‬ﺑﻭﺻ ﻪ ﻭﺍﺭﺗﻔ ﺎﻉ ‪ ٤٫٦‬ﺑﻭﺻ ﻪ ﻟﻠﺗﺭﺑ ﻪ‬
‫ﺍﻟﺧﺷﻧﻪ )ﻁﺭﻳﻘﻪ )ﺝ((‪ ،‬ﺣﻠﻘﻪ ﻣﻌﺩﻧﻳﻪ ﻭﻗﺎﻋﺩﻩ ﺷﻛﻝ )‪.(١-١١‬‬
‫‪ ‬ﻣﻁﺭﻗ ﻪ ﺗ ﺯﻥ ‪ ١٠‬ﺭﻁ ﻝ ﺗﺳ ﻘﻁ ﺳ ﻘﻭﻁ ﺣ ﺭ ﺗﺣ ﺕ ﺗ ﺎﺛﻳﺭ ﻭﺯﻧﻬ ﺎ ﻣ ﻥ‬
‫ﺍﺭﺗﻔﺎﻉ ‪ ١٨‬ﺑﻭﺻﻪ‪.‬‬
‫ﺷﻛﻝ )‪ (١-١٠‬ﺍﻟﻘﺎﻟﺏ ﻭﺍﻟﻘﺎﻋﺩﻩ ﻭﺍﻟﺣﻠﻘﻪ ﺍﻟﻣﻌﺩﻧﻳﻪ ‪ ‬‬
‫ﺍﻟﻌﻳﻧﻪ ﺍﻟﻣﺩﻣﻭﻗﻪ ﻣﻥ ﺍﻟﻘﺎﻟﺏ‪.‬‬ ‫‪ ‬ﺟﻬ ﺎﺯ ﻻﺳ ﺗﺧﺭﺍﺝ‬
‫‪ ‬ﻣﻳﺯﺍﻥ ﺩﻗﺗﻪ ﺍ ﺟﻡ‪.‬‬
‫‪ ‬ﻓﺭﻥ‪ ،‬ﻗﺎﺩﺭ ﻟﻠﺣﻔﺎﻅ ﻋﻠﻲ ﺩﺭﺟﻪ ﺍﻟﺣﺭﺍﻩ ﻋﻧﺩ )‪ (٥ ± ١١٠‬ﺩﺭﺟﻪ ﻣﺋﻭﻳﻪ‪  .‬‬
‫‪ ‬ﺍﻟﻣﻧﺎﺧ ﻝ ﺍﻟﻣﺳ ﺗﺧﺩﻣﻪ ﻓ ﻲ ﻓﺻ ﻝ ﺍﻟﻌﻳﻧ ﻪ‪ ،‬ﺍﻟﻣﻧﺧ ﻝ ﺭﻗ ﻡ ‪ ،٤‬ﺍﻟﻣﻧﺧ ﻝ ‪ ٣/٨‬ﺑﻭﺻ ﻪ ﻭ‬
‫ﺍﻟﻣﻧﺧﻝ ‪ ٣/٤‬ﺑﻭﺻﻪ ‪ ‬‬
‫ﺧﻁﻭﺍﺕ ﺍﻟﺗﺟﺭﺑﻪ‪:‬‬ ‫‪‬‬
‫‪ -١‬ﺗﻌﻳﻳﻥ ﻧﺳﺑﻪ ﺍﻟﻣﺣﺟﻭﺯ ﻣﻥ ﻭﺯﻥ ﺍﻟﻌﻧﻳﻪ ﻋﻠﻲ ﺍﻟﻣﻧﺧﻝ ﺭﻗﻡ ‪ ،٤‬ﺍﻟﻣﻧﺧﻝ ‪ ٣/٨‬ﺑﻭﺻ ﻪ‬
‫ﻭﺍﻟﻣﻧﺧﻝ ‪ ٣/٤‬ﺑﻭﺻﻪ ﻻﺧﺗﻳﺎﺭ ﺍﻟﻁﺭﻳﻘﻪ ﺍﻟﻣﺳﺗﺧﺩﻣﻪ ﻓﻲ ﺍﻻﺧﺗﺑﺎﺭ )ﻁﺭﻳﻘﻪ)ﺃ(‪ ،‬ﻁﺭﻳﻘ ﻪ )ﺏ(‪،‬‬
‫ﻁﺭﻳﻘﻪ )ﺝ((‪  .‬‬
‫ﺷﻛﻝ )‪ (٢-١٠‬ﺗﺭﻛﻳﺏ ﺍﻟﻘﺎﻟﺏ ﻭﺍﻟﺣﻠﻘﻪ ﻭﺍﻟﻘﺎﻋﺩﻩ ‪ ‬‬ ‫‪ -٢‬ﻳﺗﻡ ﺗﺟﻬﻳﺯ ﻋﻳﻧﻪ ﺍﻻﺧﺗﺑﺎﺭ ﺍﻟﺗﻲ ﺗ ﺯﻥ ‪ ١٦‬ﻛﺟ ﻡ ﻓ ﻲ ﺣﺎﻟ ﻪ ﺍﻟﻁ ﺭﻳﻘﻳﺗﻥ )ﺃ(‪) ،‬ﺏ( ﻭ‬
‫‪ ٢٩‬ﻛﺟﻡ ﻓﻲ ﺣﺎﻟﻪ ﺍﻟﻁﺭﻳﻘﻪ )ﺝ(‪  .‬‬
‫‪ -٣‬ﺗﻌﻳﻳﻥ ﻭﺯﻥ ﺍﻟﻘﺎﻟﺏ ﺍﻟﻣﺳﺗﺧﺩﻡ ﻭﻫﻭ ﻓﺎﺭﻍ ﻻﻗﺭﺏ ﺟﺭﺍﻡ‪ ،‬ﻳﺗﻡ ﺗﺛﺑﻳﺕ ﺍﻟﻘﺎﻟﺏ ﻋﻠﻲ ﺍﻟﻘﺎﻋ ﺩﻩ‬
‫ﺍﻟﻣﻌﺩﻧﻳﻪ ﻭﻭﺿﻊ ﺍﻟﺣﻠﻘﻪ ﺍﻟﻣﻌﺩﻧﻳﻪ )‪ (Extension Collar‬ﻋﻠﻲ ﺍﻟﻘﺎﻟﺏ‪  .‬‬
‫‪ -٤‬ﻳﺗﻡ ﺗﻌﻳﻳﻥ ﺍﻟﻣﺣﺗﻭﻱ ﺍﻟﺭﻁﻭﺑﻲ ﻟﻌﻳﻧﻪ ﺍﻻﺧﺗﺑﺎﺭ‪ .‬ﻭﺗﺟﻬﻳﺯ ﻋﻠﻲ ﺍﻻﻗ ﻝ ‪ ٥‬ﻋﻳﻧ ﺎﺕ ﺑﻣﺣﺗ ﻭﻱ‬
‫ﺭﻁﻭﺑﻲ ﻣﺧﺗﻠﻑ‪ .‬ﺗﺟﻬﻳﺯ ﻋﻳﻧﻪ ﺑﻣﺣﺗﻭﻱ ﺭﻁﻭﺑﻲ ﻗﺭﻳﺏ ﻣﻥ ﺍﻟﻣﺣﺗﻭﻱ ﺍﻟﺭﻁﻭﺑﻲ ﺍﻻﻣﺛﻝ‬
‫ﻭﻋﻳﻧﺗﻳﻥ ﻓﻲ ﺍﻟﺟﺎﻧﺏ ﺍﻟﺟﺎﻑ ﻭﻋﻳﻧﺗﻳﻥ ﻓﻲ ﺍﻟﺟﺎﻧﺏ ﺍﻟﺭﻁﺏ‪  .‬‬
‫‪ -٥‬ﻭﺿ ﻊ ﺍﻟﻌﻳﻧ ﻪ ﻓ ﻲ ﺍﻟﻘﺎﻟ ﺏ ﺑﻌ ﺩ ﺧﻠﻁﻬ ﺎ ﺟﻳ ﺩﺍ ﻣ ﻊ ﺍﻟﻣ ﺎء ﻟﻠﻭﺻ ﻭﻝ ﺍﻟ ﻲ ﺧﻠ ﻳﻁ ﻣﺗﻣﺎﺳ ﻙ‬
‫ﻭﺩﻣﻛﻬﺎ ﻋﻠﻲ ﻁﺑﻘﺎﺕ )ﺧﻣﺱ ﻁﺑﻘ ﺎﺕ( ﺑﻭﺍﺳ ﻁﻪ ﻣﻁﺭﻗ ﻪ ﺗ ﺯﻥ ‪ ١٠‬ﺭﻁ ﻝ ﺗﺳ ﻘﻁ ﺳ ﻘﻭﻁ‬
‫ﺣﺭ ﺗﺣﺕ ﺗﺎﺛﻳﺭ ﻭﺯﻧﻬﺎ ﻣﻥ ﺍﺭﺗﻔﺎﻉ ‪ ١٨‬ﺑﻭﺻﻪ‪  .‬‬
‫‪ -٦‬ﺗﺳ ﻭﻳﻪ ﺳ ﻁﺢ ﺍﻟﻌﻳﻧ ﻪ ﺟﻳ ﺩﺍ ﺷ ﻛﻝ )‪ ،(٤-١١‬ﺗﻌﻳ ﻳﻥ ﻭﺯﻥ ﺍﻟﻘﺎﻟ ﺏ ﻭﺍﻟﻌﻳﻧ ﻪ ﺑﻌ ﺩ ﺍﻟ ﺩﻣﻙ‬
‫ﻻﻗ ﺭﺏ ﺟ ﺭﺍﻡ‪ ،‬ﺍﺯﺍﻟ ﻪ ﺍﻟﻣ ﻭﺍﺩ ﻣ ﻥ ﺍﻟﻘﺎﻟ ﺏ ﻭﺍﺧ ﺫ ﻋﻳﻧ ﻪ ﻣ ﻥ ﻣﻧﺗﺻ ﻑ ﺍﻟﻘﺎﻟ ﺏ ﻟﺗﻌﻳ ﻳﻥ‬
‫ﺍﻟﻣﺣﺗﻭﻱ ﺍﻟﺭﻁﻭﺑﻲ ﻟﻬﺎ‪  ,‬‬
‫‪ -٧‬ﺗﻛﺭﺍﺭ ﺍﻟﺧﻁﻭﻩ ﺍﻟﺳﺎﺑﻘﻪ ﻟﻠﻌﻳﻧﺎﺕ ﺍﻻﺧﺭﻱ ﻭﺗﺳﺟﻳﻝ ﺍﻟﻘﺭﺍءﺍﺕ ‪ ‬‬
‫‪ ‬ﺍﻟﻧﺗﺎﺋﺞ‪  :‬‬
‫‪ -١‬ﻳﺗﻡ ﺣﺳﺎﺏ ﺍﻟﻛﺛﺎﻓﻪ ﺍﻟﺭﻁﺑﻪ ﻟﻠﻌﻳﻧﺎﺕ ﺍﻟﺧﻣﺳﻪ‪  :‬‬

‫𝑊‬ ‫𝑊‬
‫‪γ‬‬
‫𝑙𝑜𝑉‬
‫ﺷﻛﻝ )‪ (٣-١٠‬ﺩﻣﻙ ﺍﻟﻌﻳﻧﻪ ﺑﻭﺍﺳﻁﻪ‬
‫ﻣﻁﺭﻗﻪ ﻣﻳﻛﺎﻧﻳﻛﻳﻪ ‪ ‬‬ ‫ﺣﻳﺙ‪:‬‬

‫ﺑﻌﺩ ﺍﻟﺩﻣﻙ‪.‬‬ ‫‪ :W2‬ﻭﺯﻥ ﺍﻟﻘﺎﻟ ﺏ ﻭﺍﻟﻌﻳﻧ ﻪ‬


‫‪ :W1‬ﻭﺯﻥ ﺍﻟﻘﺎﻟﺏ ﻓﺎﺭﻏﺎ‪.‬‬
‫‪ :Vol‬ﺣﺟﻡ ﺍﻟﻘﺎﻟﺏ‪.‬‬
‫ﺍﻟﺭﻁﻭﺑﻲ ﻟﻠﻌﻳﻧﺎﺕ‪  :‬‬ ‫‪ -٢‬ﺗﻌﻳ ﻳﻥ ﺍﻟﻣﺣﺗ ﻭﻱ‬
‫𝑊‬ ‫𝑊‬
‫𝑊‬
‫𝑊‬
‫‪ :W3‬ﻭﺯﻥ ﺍﻟﻌﻳﻧﻪ ﺍﻟﻣﺑﺗﻠﻪ‬
‫‪ :W1‬ﻭﺯﻥ ﺍﻟﻌﻳﻧﻪ ﺑﻌﺩ ﺗﺟﻔﻳﻔﻬﺎ ﻓﻲ ﺍﻟﻔﺭﻥ‪.‬‬
‫ﺷﻛﻝ )‪ (٤-١٠‬ﺗﺳﻭﻳﻪ ﺳﻁﺢ ﺍﻟﻌﻳﻧﻪ ‪ ‬‬

‫‪ -٣‬ﺣﺳﺎﺏ ﺍﻟﻛﺛﺎﻓﻪ ﺍﻟﺟﺎﻓﻪ ﻟﻠﻌﻳﻧﺎﺕ‪  :‬‬


‫‪γ‬‬
‫‪γ‬‬
‫𝑊 ‪1‬‬
‫‪ -٤‬ﺭﺳ ﻡ ﻋﻼﻗ ﻪ ﺑ ﻳﻥ ﺍﻟﻛﺛﺎﻓ ﻪ ﺍﻟﺟﺎﻓ ﻪ )ﺍﻟﻣﺣ ﻭﺭ ﺍﻟﺭﺍﺳ ﻲ ﻭﺍﻟﻣﺣﺗ ﻭﻱ‬
‫ﺍﻟﺭﻁﻭﺑﻲ(‪  .‬‬

‫ﺷﻛﻝ )‪ (٥-١٠‬ﺍﻟﻌﻼﻗﻪ ﺑﻳﻥ ﺍﻟﻣﺣﺗﻭﻱ‬


‫ﺍﻟﺭﻁﻭﺑﻲ ﻭﺍﻟﻛﺛﺎﻓﻪ ﺍﻟﺟﺎﻓﻪ ‪ ‬‬
Modified Proctor of Soil and Aggregate 

% Retain on Sieve #4  =   
% Retain on 3/8 Sieve  =   
% Retain on 3/4 Sieve  =   
Method Used   =   
Calculate Water Content of Field Soil Sample 
Wt. of wet Soil   A =    gm 
Wt. of Dry soil   B =    gm 
(A‐B)/B 
Water Content  Wc = 
   
Calculate Water Content of Specimens: 
Wt. of Pan  Wt. of Pan& Spec.  Wt. of Spec.  Wt. of Dry Spec.  Water Content 
Spec. ID 
(gm)  (gm)  (gm)  (gm)  (gm) 
Spec. 1           
Spec. 2           
Spec. 3           
Spec. 4           
Spec. 5           
Calculate Dry Density of Specimens: 
Specimen  Wt. of  Vol. of  Wt. of Mold and  Wt. of  Wet Density  Water  Dry Density 
ID  Mold  mold  Specimen  Specimen  (Ywet)  Content  (YDry) 
Spec. 1           
Spec. 2           
Spec. 3               
Spec. 4           
Spec. 5           
‫ﺗﺟﺭﺑﻪ ﺭﻗﻡ ‪-١١-‬‬
‫ﺧﺻﺎﺋﺹ ﺍﻟﺗﺭﺑﻪ ﺍﻟﻣﺩﻣﻭﻛﻪ ﺑﺎﺳﺗﺧﺩﺍﻡ ﺍﻟﺑﺭﻭﻛﺗﻭﺭ ﺍﻟﻘﻳﺎﺳﻲ‬
‫‪Laboratory Compaction Characteristics of Soil Using Standard Effort‬‬
‫‪  ASTM D1557‬‬
‫‪ ‬ﺍﻟﻐﺭﺽ‪:‬‬
‫ﻳﻐﻁﻲ ﻫﺫﺍ ﺍﻻﺧﺗﺑﺎﺭ ﻁﺭﻕ ﺍﻟﺩﻣﻙ ﺍﻟﻣﻌﻣﻠﻳﻪ ﺍﻟﻣﺳﺗﺧﺩﻣﻪ ﻓﻲ ﺗﻌﻳﻳﻥ ﺍﻟﻌﻼﻗﻪ ﺑ ﻳﻥ ﺍﻟﻣﺣﺗ ﻭﻱ ﺍﻟﺭﻁ ﻭﺑﻲ ﻭﺍﻟﻛﺛﺎﻓ ﻪ ﺍﻟﺟﺎﻓ ﻪ ﻟﻠﺗﺭﺑ ﻪ )ﻣﻧﺣﻧ ﻲ‬
‫ﺍﻟﺩﻣﻙ(‪ ،‬ﺗﺩﻣﻙ ﺍﻟﻌﻳﻧﺎﺕ ﻓ ﻲ ﻗﺎﻟ ﺏ ﻗﻳﺎﺳ ﻲ ﺑﻘﻁ ﺭ ‪ ٤‬ﺍﻭ ‪ ٦‬ﺑﻭﺻ ﻪ ﺑﻭﺍﺳ ﻁﻪ ﻣﻁﺭﻗ ﻪ ﺗ ﺯﻥ ‪ ٥٫٥‬ﺭﻁ ﻝ ﺗﺳ ﻘﻁ ﺳ ﻘﻭﻁ ﺣ ﺭ ﺗﺣ ﺕ ﺗ ﺎﺛﻳﺭ‬
‫ﻭﺯﻧﻬﺎ ﻣﻥ ﺍﺭﺗﻔﺎﻉ ‪ ١٠‬ﺑﻭﺻﻪ‪.‬‬
‫ﻳﺳﻣﺢ ﺑﺎﺟﺭﺍء ﻫﺫﺍ ﺍﻻﺧﺗﺑﺎﺭ ﻋﻠﻲ ﺍﻟﻣﻭﺍﺩ ﺍﻟﻣﺣﺗﻭﺍﻩ ﻋﻠﻲ ‪ %٣٠‬ﺍﻭ ﺍﻗﻝ ﻣﻥ ﻭﺯﻧﻬﺎ ﻣﺣﺟﻭﺯﻩ ﻋﻠﻲ ﺍﻟﻣﻧﺧﻝ )‪ (٣/٤‬ﺑﻭﺻﻪ‪.‬‬
‫ﻁﺭﻳﻘﻪ )ﺝ(‬ ‫ﻁﺭﻳﻘﻪ )ﺏ(‬ ‫ﻁﺭﻳﻘﻪ )ﺃ(‬
‫ﻗﻁﺭ ‪ ٦‬ﺑﻭﺻﻪ‬ ‫ﻗﻁﺭ ‪ ٤‬ﺑﻭﺻﻪ‬ ‫ﻗﻁﺭ ‪ ٤‬ﺑﻭﺻﻪ‬ ‫ﺍﻟﻘﺎﻟﺏ ﺍﻟﻣﺳﺗﺧﺩﻡ‬
‫ﺍﻟﻣ ﺎﺭ ﻣ ﻥ ﺍﻟﻣﻧﺧ ﻝ ‪ ٣/٤‬ﺑﻭﺻ ﻪ‪ .‬ﻓ ﻲ‬ ‫ﺍﻟﻣﺎﺭ ﻣﻥ ﺍﻟﻣﻧﺧﻝ ‪ ٣/٨‬ﺑﻭﺻ ﻪ‪ .‬ﻓ ﻲ ﺣﺎﻟ ﻪ‬ ‫ﺍﻟﻣ ﺎﺭ ﻣ ﻥ ﺍﻟﻣﻧﺧ ﻝ ﺭﻗ ﻡ ‪٤‬‬ ‫ﺍﻟﻣﻭﺍﺩ ﺍﻟﻣﺳﺗﺧﺩﻣﻪ‬
‫ﺣﺎﻟ ﻪ ﺯﻳ ﺎﺩﻩ ﻧﺳ ﺑﻪ ﺍﻟﻣ ﻭﺍﺩ ﺍﻟﻣﺣﺟ ﻭﺯﻩ‬ ‫ﺯﻳ ﺎﺩﻩ ﻧﺳ ﺑﻪ ﺍﻟﻣ ﻭﺍﺩ ﺍﻟﻣﺣﺟ ﻭﺯﻩ ﻋﻠ ﻲ‬ ‫ﺑﺣﻳﺙ ﻳﻛ ﻭﻥ ﺍﻟﻣﺣﺟ ﻭﺯ ﻋﻠ ﻲ‬
‫ﻋﻠ ﻲ ﺍﻟﻣﻧﺧ ﻝ ‪ ٣/٨‬ﺑﻭﺻ ﻪ ﺍﻛﺑ ﺭ ﻣ ﻥ‬ ‫ﺍﻟﻣﻧﺧ ﻝ ﺭﻗ ﻡ ‪ ٤‬ﻋ ﻥ ‪ %٢٠‬ﻭﺍﻟﻣﺣﺟ ﻭﺯ‬ ‫ﺍﻟﻣﻧﺧ ﻝ ﺭﻗ ﻡ ‪ ٤‬ﺍﻗ ﻝ ﻣ ﻥ ﺍﻭ‬
‫‪ %٢٠‬ﻭﺍﻟﻣﺣﺟ ﻭﺯ ﻋﻠ ﻲ ﺍﻟﻣﻧﺧ ﻝ ‪٣/٤‬‬ ‫ﻋﻠ ﻲ ﺍﻟﻣﻧﺧ ﻝ ‪ ٣/٨‬ﺑﻭﺻ ﻪ ﺍﻗ ﻝ ﻣ ﻥ‬ ‫ﻳﺳ ﺎﻭﻱ ‪ %٢٠‬ﻣ ﻥ ﻭﺯﻥ‬
‫ﺑﻭﺻﻪ ﺍﻗﻝ ﻣﻥ ‪%٣٠‬‬ ‫‪.%٢٠‬‬ ‫ﺍﻟﻌﻳﻧﻪ‪.‬‬
‫‪ ٥‬ﻁﺑﻘﺎﺕ‬ ‫‪ ٥‬ﻁﺑﻘﺎﺕ‬ ‫‪ ٥‬ﻁﺑﻘﺎﺕ‬ ‫ﻋﺩﺩ ﺍﻟﻁﺑﻘﺎﺕ‬
‫‪ ٥٦‬ﺩﻗﻪ‪/‬ﻁﺑﻘﻪ‬ ‫‪ ٢٥‬ﺩﻗﻪ‪/‬ﻁﺑﻘﻪ‬ ‫‪ ٢٥‬ﺩﻗﻪ‪/‬ﻁﺑﻘﻪ‬ ‫ﻋﺩﺩ ﺍﻟﺩﻗﺎﺕ‬

‫‪ ‬ﺍﻻﻫﻣﻳﻪ ﻭﺍﻻﺳﺗﺧﺩﺍﻡ‪:‬‬
‫ﺗﺩﻣﻙ ﻁﺑﻘﺎﺕ ﺍﻟﺭﺻﻑ )ﻁﺑﻘﻪ ﺍﻻﺳﺎﺱ‪ ،‬ﺍﻻﺳﺎﺱ ﺍﻟﻣﺳﺎﻋﺩ‪ ،‬ﻭﻁﺑﻘﻪ ﺍﻟﺗﺎﺳ ﻳﺱ( ﻟﻠﻭﺻ ﻭﻝ ﻻﻗﺻ ﻲ ﻛﺛﺎﻓ ﻪ ﻟﻠﺣﺻ ﻭﻝ ﻋﻠ ﻲ ﺍﻟﺧﺻ ﺎﺋﺹ‬
‫ﺍﻟﻬﻧﺩﺳﻳﻪ ﺍﻟﻣﻁﻠﻭﺑﻪ ﻣﻥ ﺣﻳﺙ )ﻣﻘﺎﻭﻣﻪ ﺍﻟﻘﺹ‪ ،‬ﻗﺎﺑﻠﻳﻪ ﺍﻧﺿﻐﺎﻁ ﺍﻟﺗﺭﺑﻪ ﺍﻭ ﻧﻔﺎﺫﻳﻪ ﺍﻟﺗﺭﺑﻪ(‪.‬‬
‫ﺣﺳﺎﺏ ﻧﺳﺑﻪ ﺍﻟﺩﻣﻙ ﻭﻣﺣﺗﻭﻱ ﺍﻟﺭﻁﻭﺑﻪ ﺍﻟﻼﺯﻡ ﻟﺗﺣﻘﻳﻖ ﺍﻟﺧﺻﺎﺋﺹ ﺍﻟﻣﻁﻠﻭﺑﻪ‪.‬‬
‫‪ ‬ﺍﻻﺟﻬﺯﻩ‪  :‬‬
‫‪ ‬ﻗﺎﻟ ﺏ ﻗﻳﺎﺳ ﻲ ﺑﻘﻁ ﺭ ‪ ٤‬ﺑﻭﺻ ﻪ ﻭﺍﺭﺗﻔ ﺎﻉ ‪ ٤٫٦‬ﺑﻭﺻ ﻪ ﻟﻠﺗﺭﺑ ﻪ ﺍﻟﻧﺎﻋﻣ ﻪ‬
‫)ﻁﺭﻳﻘ ﻪ )ﺃ(‪) ،‬ﺏ(( ﻭﺑﻘﻁ ﺭ ‪ ٦‬ﺑﻭﺻ ﻪ ﻭﺍﺭﺗﻔ ﺎﻉ ‪ ٤٫٦‬ﺑﻭﺻ ﻪ ﻟﻠﺗﺭﺑ ﻪ‬
‫ﺍﻟﺧﺷﻧﻪ )ﻁﺭﻳﻘﻪ )ﺝ((‪ ،‬ﺣﻠﻘﻪ ﻣﻌﺩﻧﻳﻪ ﻭﻗﺎﻋﺩﻩ ﺷﻛﻝ )‪.(١-١٢‬‬
‫‪ ‬ﻣﻁﺭﻗ ﻪ ﺗ ﺯﻥ ‪ ٥٫٥‬ﺭﻁ ﻝ ﺗﺳ ﻘﻁ ﺳ ﻘﻭﻁ ﺣ ﺭ ﺗﺣ ﺕ ﺗ ﺎﺛﻳﺭ ﻭﺯﻧﻬ ﺎ ﻣ ﻥ‬
‫ﺍﺭﺗﻔﺎﻉ ‪ ١٠‬ﺑﻭﺻﻪ‪.‬‬
‫ﺷﻛﻝ )‪ (١-١١‬ﺍﻟﻘﺎﻟﺏ ﻭﺍﻟﻘﺎﻋﺩﻩ ﻭﺍﻟﺣﻠﻘﻪ ﺍﻟﻣﻌﺩﻧﻳﻪ ‪ ‬‬
‫ﺍﻟﻌﻳﻧﻪ ﺍﻟﻣﺩﻣﻭﻗﻪ ﻣﻥ ﺍﻟﻘﺎﻟﺏ‪.‬‬ ‫‪ ‬ﺟﻬ ﺎﺯ ﻻﺳ ﺗﺧﺭﺍﺝ‬
‫‪ ‬ﻣﻳﺯﺍﻥ ﺩﻗﺗﻪ ﺍ ﺟﻡ‪.‬‬
‫‪ ‬ﻓﺭﻥ‪ ،‬ﻗﺎﺩﺭ ﻟﻠﺣﻔﺎﻅ ﻋﻠﻲ ﺩﺭﺟﻪ ﺍﻟﺣﺭﺍﻩ ﻋﻧﺩ )‪ (٥ ± ١١٠‬ﺩﺭﺟﻪ ﻣﺋﻭﻳﻪ‪  .‬‬
‫‪ ‬ﺍﻟﻣﻧﺎﺧ ﻝ ﺍﻟﻣﺳ ﺗﺧﺩﻣﻪ ﻓ ﻲ ﻓﺻ ﻝ ﺍﻟﻌﻳﻧ ﻪ‪ ،‬ﺍﻟﻣﻧﺧ ﻝ ﺭﻗ ﻡ ‪ ،٤‬ﺍﻟﻣﻧﺧ ﻝ ‪ ٣/٨‬ﺑﻭﺻ ﻪ ﻭ‬
‫ﺍﻟﻣﻧﺧﻝ ‪ ٣/٤‬ﺑﻭﺻﻪ‪  .‬‬
‫ﺧﻁﻭﺍﺕ ﺍﻟﺗﺟﺭﺑﻪ‪:‬‬ ‫‪‬‬
‫‪ -٨‬ﺗﻌﻳﻳﻥ ﻧﺳﺑﻪ ﺍﻟﻣﺣﺟﻭﺯ ﻣﻥ ﻭﺯﻥ ﺍﻟﻌﻧﻳﻪ ﻋﻠﻲ ﺍﻟﻣﻧﺧﻝ ﺭﻗﻡ ‪ ،٤‬ﺍﻟﻣﻧﺧﻝ ‪ ٣/٨‬ﺑﻭﺻ ﻪ‬
‫ﻭﺍﻟﻣﻧﺧﻝ ‪ ٣/٤‬ﺑﻭﺻﻪ ﻻﺧﺗﻳﺎﺭ ﺍﻟﻁﺭﻳﻘﻪ ﺍﻟﻣﺳﺗﺧﺩﻣﻪ ﻓﻲ ﺍﻻﺧﺗﺑﺎﺭ )ﻁﺭﻳﻘﻪ)ﺃ(‪ ،‬ﻁﺭﻳﻘ ﻪ )ﺏ(‪،‬‬
‫ﻁﺭﻳﻘﻪ )ﺝ((‪  .‬‬
‫ﺷﻛﻝ )‪ (٢-١١‬ﺗﺭﻛﻳﺏ ﺍﻟﻘﺎﻟﺏ ﻭﺍﻟﺣﻠﻘﻪ ﻭﺍﻟﻘﺎﻋﺩﻩ ‪ ‬‬ ‫‪ -٩‬ﻳﺗﻡ ﺗﺟﻬﻳﺯ ﻋﻳﻧﻪ ﺍﻻﺧﺗﺑﺎﺭ ﺍﻟﺗﻲ ﺗ ﺯﻥ ‪ ١٦‬ﻛﺟ ﻡ ﻓ ﻲ ﺣﺎﻟ ﻪ ﺍﻟﻁ ﺭﻳﻘﻳﺗﻥ )ﺃ(‪) ،‬ﺏ( ﻭ‬
‫‪ ٢٩‬ﻛﺟﻡ ﻓﻲ ﺣﺎﻟﻪ ﺍﻟﻁﺭﻳﻘﻪ )ﺝ(‪  .‬‬
‫‪ -١٠‬ﺗﻌﻳﻳﻥ ﻭﺯﻥ ﺍﻟﻘﺎﻟﺏ ﺍﻟﻣﺳﺗﺧﺩﻡ ﻭﻫﻭ ﻓﺎﺭﻍ ﻻﻗﺭﺏ ﺟﺭﺍﻡ‪ ،‬ﻳﺗﻡ ﺗﺛﺑﻳﺕ ﺍﻟﻘﺎﻟﺏ ﻋﻠﻲ ﺍﻟﻘﺎﻋ ﺩﻩ‬
‫ﺍﻟﻣﻌﺩﻧﻳﻪ ﻭﻭﺿﻊ ﺍﻟﺣﻠﻘﻪ ﺍﻟﻣﻌﺩﻧﻳﻪ )‪ (Extension Collar‬ﻋﻠﻲ ﺍﻟﻘﺎﻟﺏ‪  .‬‬
‫‪ -١١‬ﻳﺗﻡ ﺗﻌﻳﻳﻥ ﺍﻟﻣﺣﺗﻭﻱ ﺍﻟﺭﻁﻭﺑﻲ ﻟﻌﻳﻧﻪ ﺍﻻﺧﺗﺑﺎﺭ‪ .‬ﻭﺗﺟﻬﻳﺯ ﻋﻠﻲ ﺍﻻﻗ ﻝ ‪ ٥‬ﻋﻳﻧ ﺎﺕ ﺑﻣﺣﺗ ﻭﻱ‬
‫ﺭﻁﻭﺑﻲ ﻣﺧﺗﻠﻑ‪ .‬ﺗﺟﻬﻳﺯ ﻋﻳﻧﻪ ﺑﻣﺣﺗﻭﻱ ﺭﻁﻭﺑﻲ ﻗﺭﻳﺏ ﻣﻥ ﺍﻟﻣﺣﺗﻭﻱ ﺍﻟﺭﻁﻭﺑﻲ ﺍﻻﻣﺛﻝ‬
‫ﻭﻋﻳﻧﺗﻳﻥ ﻓﻲ ﺍﻟﺟﺎﻧﺏ ﺍﻟﺟﺎﻑ ﻭﻋﻳﻧﺗﻳﻥ ﻓﻲ ﺍﻟﺟﺎﻧﺏ ﺍﻟﺭﻁﺏ‪  .‬‬
‫‪ -١٢‬ﻭﺿ ﻊ ﺍﻟﻌﻳﻧ ﻪ ﻓ ﻲ ﺍﻟﻘﺎﻟ ﺏ ﺑﻌ ﺩ ﺧﻠﻁﻬ ﺎ ﺟﻳ ﺩﺍ ﻣ ﻊ ﺍﻟﻣ ﺎء ﻟﻠﻭﺻ ﻭﻝ ﺍﻟ ﻲ ﺧﻠ ﻳﻁ ﻣﺗﻣﺎﺳ ﻙ‬
‫ﻭﺩﻣﻛﻬﺎ ﻋﻠﻲ ﻁﺑﻘﺎﺕ )ﺧﻣﺱ ﻁﺑﻘﺎﺕ( ﺑﻭﺍﺳﻁﻪ ﻣﻁﺭﻗﻪ ﺗ ﺯﻥ ‪ ٥٫٥‬ﺭﻁ ﻝ ﺗﺳ ﻘﻁ ﺳ ﻘﻭﻁ‬
‫ﺣﺭ ﺗﺣﺕ ﺗﺎﺛﻳﺭ ﻭﺯﻧﻬﺎ ﻣﻥ ﺍﺭﺗﻔﺎﻉ ‪ ١٠‬ﺑﻭﺻﻪ‪  .‬‬
‫‪ -١٣‬ﺗﺳ ﻭﻳﻪ ﺳ ﻁﺢ ﺍﻟﻌﻳﻧ ﻪ ﺟﻳ ﺩﺍ ﺷ ﻛﻝ )‪ ،(٤-١٢‬ﺗﻌﻳ ﻳﻥ ﻭﺯﻥ ﺍﻟﻘﺎﻟ ﺏ ﻭﺍﻟﻌﻳﻧ ﻪ ﺑﻌ ﺩ ﺍﻟ ﺩﻣﻙ‬
‫ﻻﻗ ﺭﺏ ﺟ ﺭﺍﻡ‪ ،‬ﺍﺯﺍﻟ ﻪ ﺍﻟﻣ ﻭﺍﺩ ﻣ ﻥ ﺍﻟﻘﺎﻟ ﺏ ﻭﺍﺧ ﺫ ﻋﻳﻧ ﻪ ﻣ ﻥ ﻣﻧﺗﺻ ﻑ ﺍﻟﻘﺎﻟ ﺏ ﻟﺗﻌﻳ ﻳﻥ‬
‫ﺍﻟﻣﺣﺗﻭﻱ ﺍﻟﺭﻁﻭﺑﻲ ﻟﻬﺎ‪  ,‬‬
‫‪ -١٤‬ﺗﻛﺭﺍﺭ ﺍﻟﺧﻁﻭﻩ ﺍﻟﺳﺎﺑﻘﻪ ﻟﻠﻌﻳﻧﺎﺕ ﺍﻻﺧﺭﻱ ﻭﺗﺳﺟﻳﻝ ﺍﻟﻘﺭﺍءﺍﺕ ‪ ‬‬
‫‪ ‬ﺍﻟﻧﺗﺎﺋﺞ‪  :‬‬
‫‪ -٥‬ﻳﺗﻡ ﺣﺳﺎﺏ ﺍﻟﻛﺛﺎﻓﻪ ﺍﻟﺭﻁﺑﻪ ﻟﻠﻌﻳﻧﺎﺕ ﺍﻟﺧﻣﺳﻪ‪  :‬‬

‫𝑊‬ ‫𝑊‬
‫‪γ‬‬
‫𝑙𝑜𝑉‬
‫ﺷﻛﻝ )‪ (٣-١١‬ﺩﻣﻙ ﺍﻟﻌﻳﻧﻪ ﺑﻭﺍﺳﻁﻪ‬
‫ﻣﻁﺭﻗﻪ ﻣﻳﻛﺎﻧﻳﻛﻳﻪ ‪ ‬‬ ‫ﺣﻳﺙ‪:‬‬

‫ﺑﻌﺩ ﺍﻟﺩﻣﻙ‪.‬‬ ‫‪ :W2‬ﻭﺯﻥ ﺍﻟﻘﺎﻟ ﺏ ﻭﺍﻟﻌﻳﻧ ﻪ‬


‫‪ :W1‬ﻭﺯﻥ ﺍﻟﻘﺎﻟﺏ ﻓﺎﺭﻏﺎ‪.‬‬
‫‪ :Vol‬ﺣﺟﻡ ﺍﻟﻘﺎﻟﺏ‪.‬‬
‫ﺍﻟﺭﻁﻭﺑﻲ ﻟﻠﻌﻳﻧﺎﺕ‪  :‬‬ ‫‪ -٦‬ﺗﻌﻳ ﻳﻥ ﺍﻟﻣﺣﺗ ﻭﻱ‬
‫𝑊‬ ‫𝑊‬
‫𝑊‬
‫𝑊‬
‫‪ :W3‬ﻭﺯﻥ ﺍﻟﻌﻳﻧﻪ ﺍﻟﻣﺑﺗﻠﻪ‬
‫‪ :W1‬ﻭﺯﻥ ﺍﻟﻌﻳﻧﻪ ﺑﻌﺩ ﺗﺟﻔﻳﻔﻬﺎ ﻓﻲ ﺍﻟﻔﺭﻥ‪.‬‬
‫ﺷﻛﻝ )‪ (٤-١١‬ﺗﺳﻭﻳﻪ ﺳﻁﺢ ﺍﻟﻌﻳﻧﻪ ‪ ‬‬

‫‪ -٧‬ﺣﺳﺎﺏ ﺍﻟﻛﺛﺎﻓﻪ ﺍﻟﺟﺎﻓﻪ ﻟﻠﻌﻳﻧﺎﺕ‪  :‬‬


‫‪γ‬‬
‫‪γ‬‬
‫𝑊 ‪1‬‬
‫‪ -٨‬ﺭﺳ ﻡ ﻋﻼﻗ ﻪ ﺑ ﻳﻥ ﺍﻟﻛﺛﺎﻓ ﻪ ﺍﻟﺟﺎﻓ ﻪ )ﺍﻟﻣﺣ ﻭﺭ ﺍﻟﺭﺍﺳ ﻲ ﻭﺍﻟﻣﺣﺗ ﻭﻱ‬
‫ﺍﻟﺭﻁﻭﺑﻲ(‪  .‬‬

‫ﺷﻛﻝ )‪ (٥-١١‬ﺍﻟﻌﻼﻗﻪ ﺑﻳﻥ ﺍﻟﻣﺣﺗﻭﻱ‬


‫ﺍﻟﺭﻁﻭﺑﻲ ﻭﺍﻟﻛﺛﺎﻓﻪ ﺍﻟﺟﺎﻓﻪ ‪ ‬‬
Modified Proctor of Soil and Aggregate 

% Retain on Sieve #4  =   
% Retain on 3/8 Sieve  =   
% Retain on 3/4 Sieve  =   
Method Used   =   
Calculate Water Content of Field Soil Sample 
Wt. of wet Soil   A =    gm 
Wt. of Dry soil   B =    gm 
(A‐B)/B 
Water Content  Wc = 
   
Calculate Water Content of Specimens: 
Wt. of Pan  Wt. of Pan& Spec.  Wt. of Spec.  Wt. of Dry Spec.  Water Content 
Spec. ID 
(gm)  (gm)  (gm)  (gm)  (gm) 
Spec. 1           
Spec. 2           
Spec. 3           
Spec. 4           
Spec. 5           
Calculate Dry Density of Specimens: 
Specimen  Wt. of  Vol. of  Wt. of Mold and  Wt. of  Wet Density  Water  Dry Density 
ID  Mold  mold  Specimen  Specimen  (Ywet)  Content  (YDry) 
Spec. 1           
Spec. 2           
Spec. 3               
Spec. 4           
Spec. 5           
‫ﺗﺟﺭﺑﻪ ﺭﻗﻡ ‪-12-‬‬
‫ﺗﺣﺿﻳﺭ ﻋﻳﻧﺔ ﺍﻟﺧﺭﺳﺎﻧﻪ ﺍﻻﺳﻔﻠﺗﻳﻪ ﺑﺎﺳﻳﺗﺧﺩﺍﻡ ﻣﺎﺭﺷﺎﻝ‬
‫‪Preparation of Asphalt Concrete specimens using the Marshall Compactor‬‬
‫‪  ASTM D1559‬‬
‫‪ ‬ﺍﻟﻐﺭﺽ ‪:‬‬
‫ﺗﺟﻬﻳﺯ ﻋﻳﻧﺔ ﺍﻟﺧﺭﺳﺎﻧﻪ ﺍﻻﺳﻔﻠﺗﻳﻪ ﺑﺎﺳﺗﺧﺩﺍﻡ ﻁﺭﻳﻘﻪ ﻣﺎﺭﺷﺎﻝ‪.‬‬
‫‪ ‬ﺍﻻﻫﻣﻳﺔ ﻭﺍﻻﺳﺗﺧﺩﻡ ‪:‬‬
‫ﺗﺳﺗﺧﺩﻡ ﻫﺫﻩ ﺍﻟﻁﺭﻳﻘﺔ ﻟﺗﺻﻣﻳﻡ ﺍﻟﺧﻠﻁﻪ ﺍﻻﺳﻔﺗﻠﻳﺔ ﺑﺎﺳﺗﺧﺩﺍﻡ ﻣﺎﺭﺷﺎﻝ ﻟﻘﻳﺎﺱ ﺧﺻﺎﺋﺻﻬﺎ‪.‬‬
‫ﺍﻻﺟﻬﺯﺓ ‪:‬‬ ‫‪‬‬
‫ﻣﻁﺭﻗﺔ ﺩﻣﻙ ﺗﺯﻥ ﺣﻭﺍﻟﻲ ‪ ٤٫٥‬ﻛﺟﻡ‪ ،‬ﻭﺗﺳﻘﻁ ﺳﻘﻭﻁ ﺣﺭ ﻣﻥ ﺍﺭﺗﻔﺎﻉ ‪ ٤٨‬ﺳﻡ‪.‬‬ ‫‪.١‬‬
‫ﻗﺎﻟﺏ ﻣﻌﺩﻧﻲ‪ ،‬ﻗﻁﺭﻩ ﺍﻟﺩﺍﺧﻠﻲ ‪ ١٠٢‬ﻣﻡ ﻭﺍﺭﺗﻔﺎﻋﻪ ‪ ٧٥‬ﻣﻡ‪ ،‬ﻗﺎﻋﺩﻩ ﻭﺣﻠﻘﻪ ﻣﻌﺩﻧﻳﺔ‬ ‫‪.٢‬‬
‫ﻁﺎﺭﺩ ﺍﻟﻌﻳﻧﺔ "ﺟﻬﺎﺯ ﻻﺧﺭﺍﺝ ﺍﻟﻌﻳﻧﺔ ﻣﻥ ﺍﻟﻘﺎﻟﺏ ﺍﻟﻣﻌﺩﻧﻲ"‪ ،‬ﻣﻠﻌﻘﺔ‪ ،‬ﻭﻋﺎء‪ ،‬ﺣﺎﻣﻝ ﺍﻟﻘﺎﻟﺏ ﻭﻓﺭﻥ‪.‬‬ ‫‪.٣‬‬
‫ﺧﻁﻭﺍ ﺍﻟﺗﺟﺭﺑﺔ ‪:‬‬ ‫‪‬‬
‫ﺣﺳﺎﺏ ﺩﺭﺟﻪ ﺣﺭﺍﺭﻩ ﺍﻟﺧﻠﻁ ﻭﺍﻟﺩﻣﻙ ﺑﺣﺙ ﺗﻛﻭﻥ ﻟﺯﻭﺟ ﻪ ﺍﻟﻣ ﺎﺩﻩ ﺍﻟﺭﺍﺑﻁ ﻪ )‪ (٢٠ ± ١٧٠‬ﺳ ﻧﺗﻲ‬ ‫‪.١‬‬
‫ﺳﺗﻭﻙ ﻟﻠﺧﻠﻁ ﻭ )‪ (٣٠ ± ٢٨٠‬ﺳﻧﺗﻲ ﺳﺗﻭﻙ ﻟﻠﺩﻣﻙ‪.‬‬
‫ﻓﺻﻝ ﺍﻟﺭﻛﺎﻡ ﻭﺗﺟﻔﻳﻔﻪ ﺣﺗﻲ ﻳﺛﺑﺕ ﻭﺯﻧﻪ‪.‬‬ ‫‪.٢‬‬
‫ﺷﻛﻝ )‪ (١-١٢‬ﻣﻁﺭﻗﺔ‬
‫ﻭﺯﻥ ﺣﻭﺍﻟﻲ ‪ ١٢٠٠‬ﺟﻡ ﻣﻥ ﺍﻟﺭﻛﺎﻡ ﺑﺣﻳﺙ ﻳﻛﻭﻥ ﺍﻟﺗﺩﺭﺝ ﻣﻁﺎﺑﻖ ﻟﻠﻣﻭﺍﺻﻔﺎﺕ‬ ‫‪.٣‬‬
‫ﻭﺿﻊ ﺍﻻﺳﻔﻠﺕ ﻭﺍﻟﺭﻛﺎﻡ ﻓﻲ ﺍﻟﻔﺭﻥ ﺣﺗﻲ ﻳﺻﻼ ﻟﺩﺭﺟﻪ ﺣ ﺭﺍﺭﻩ ﺍﻟﺧﻠ ﻁ‬ ‫‪.٤‬‬
‫)‪ ١٦٠‬ﺩﺭﺟﻪ ﻣﺋﻭﻳﻪ ﺗﻘﺭﻳﺑﺎ(‪  .‬‬
‫ﺇﺿﺎﻓﺔ ﺍﻻﺳﻔﻠﺕ ﻋﻠﻲ ﺍﻟﺭﻛﺎﻡ ﺑﺎﻟﻛﻣﻳﻪ ﺍﻟﻣﺣﺩﺩﻩ‪  .‬‬ ‫‪.٥‬‬
‫ﺧﻠﻁ ﺍﻟﺭﻛﺎﻡ ﻭﺍﻻﺳﻔﻠﺕ ﺟﻳﺩﺍ ﺣﺗﻲ ﺗﺗﻐﻠ ﻑ ﺣﺑﻳﺑ ﺎﺕ ﺍﻟﺭﻛ ﺎﻡ ﺑﺎﻻﺳ ﻔﻠﺕ‪،‬‬ ‫‪.٦‬‬
‫ﺍﻟﻘﺎﻟﺏ ﻭﺍﻟﺣﻠﻘﻪ‬ ‫ﺑﺎﺳﺗﺧﺩﺍﻡ ﺍﻟﺧﻠﻁ ﺍﻟﻳﺩﻭﻱ ﺍﻭ ﺍﻟﻣﻳﻛﺎﻧﻳﻛﻲ‪  .‬‬
‫ﻭﺿ ﻊ ﺍﻟﻭﺭﻗ ﺔ ﺩﺧ ﻝ ﺍﻟﻘﺎﻟ ﺏ‪ .‬ﺛ ﻡ ﺗﻭﺿ ﻊ ﺍﻟﻌﻳﻧ ﺔ ﻓ ﻲ ﺍﻟﻘﺎﻟ ﺏ ﺍﻟﻣﺳ ﺧﻥ‬ ‫‪.٧‬‬
‫ﻟﺩﺭﺟﻪ ﺣﺭﺍﺭﻩ ﺍﻟﺧﻠ ﻁ‪ ،‬ﻭﻏﺯﻏ ﺯﻩ ﺍﻟﻌﻳﻧ ﻪ ‪ ١٥‬ﻣ ﺭﻩ ﻋﻠ ﻲ‬
‫ﺣﺎﻣﻝ ﺍﻟﻘﺎﻟﺏ ‪ ‬‬ ‫ﺍﻟﻣﺣﻳﻁ ﻭ‪ ١٠‬ﻣﺭﺍﺕ ﻓﻲ ﺍﻟﻣﻧﺗﺻﻑ‪  .‬‬
‫ﻭﺿ ﻊ ﺍﻟﺣﻠﻘ ﻪ ﺍﻟﻣﻌﺩﻧﻳ ﻪ ﻭﺍﻟﻭﺭﻗ ﺔ )ﻭﺭﻗ ﺔ ﺗﺭﺷ ﻳﺢ ﻟﻣﻧ ﻊ‬ ‫‪.٨‬‬
‫ﺍﻟﺗﺻ ﺎﻕ ﺍﻟﻌﻳﻧ ﺔ ﺑﺎﻟﻘﺎﻟ ﺏ(‪ ،‬ﻭﻳﻭﺿ ﻊ ﺍﻟﻘﺎﻟ ﺏ ﻋﻠ ﻲ ﺍﻟﻘﺎﻋ ﺩﺓ‪ .‬ﻭﻳﺛﺑ ﺕ‬
‫ﺍﻟﻘﺎﻟ ﺏ ﺑﻭﺍﺳ ﻁﻪ ﺍﻟﺣﺎﻣ ﻝ‪ ،‬ﺗﻌ ﺭﺽ ﺍﻟﻌﻳﻧ ﺔ ﻟﻌ ﺩﻩ ﻁﺭﻗ ﺎﺕ )‪(٧٥ ، ٥٠‬‬
‫"ﻳﻌﺗﻣﺩ ﻋ ﺩﺩ ﺍﻟﻁﺭﻗ ﺎﺕ ﻋﻠ ﻲ ﺣﺟ ﻡ ﺍﻟﻣ ﺭﻭﺭ ﺍﻟﻣﺗﻭﻗ ﻊ ﻋﻠ ﻲ ﺍﻟﻁﺭﻳ ﻖ"‪.‬‬
‫ﻗﻠﺏ ﺍﻟﻘﺎﻟﺏ ﻭﺗﻌﺭﻳﺿﻪ ﻟﻧﻔﺱ ﻋﺩﺩ ﺍﻟﻁﺭﻗﺎﺕ ﻋﻠﻲ ﺍﻟﻭﺟﻪ ﺍﻻﺧﺭ‪  .‬‬
‫ﺍﻟﻌﻳﻧﺔ ﻟﺩﺭﺟﻪ ﺣﺭﺍﺭﻩ ﺍﻟﻐﺭﻓﺔ‪ ،‬ﺗﺧﺭﺝ ﺍﻟﻌﻳﻧﺔ ﻣﻥ‬ ‫ﺷﻛﻝ )‪ (٢-١٢‬ﺍﻻﺟﻬﺯﺓ ﺍﻟﻣﺳﺗﺧﺩﻣﺔ ﻓﻲ ﺍﺧﺗﺑﺎﺭ ﻣﺎﺭﺷﺎﻝ‬ ‫‪ .٩‬ﺑﻌ ﺩ ﺗﺑ ﺭﻱ‬
‫ﺑﻭﺍﺳ ﻁﻪ ﺍﺩﺍﻩ ﺍﻻﺧ ﺭﺍﺝ " ‪extruding ‬‬ ‫ﺏ‬ ‫ﺍﻟﻘﺎﻟ‬
‫‪ ."device‬ﻳﻣﻛ ﻥ ﺯﻳ ﺎﺩﻩ ﺳ ﺭﻋﻪ ﺗﺑﺭﻳ ﺩ ﺍﻟﻌﻳﻧ ﺔ ﺑﻭﺿ ﻌﻬﺎ ﻓ ﻲ ﻛ ﻳﺱ ﺑﻼﺳ ﺗﻳﻙ ﻭﻏﻣ ﺭﻩ ﻓ ﻲ ﻣﻳ ﺎﻩ ﺑ ﺎﺭﺩ‪ .‬ﺍﺯﺍﻟ ﻪ ﺍﻟﻭﺭﻗ ﻪ ﻛﻣ ﺎ ﻫ ﻭ‬
‫ﻣﻭﺿﺢ ﺑﺎﻟﺷﻛﻝ )( ‪ ‬‬
‫‪ ‬ﺍﻟﺗﻘﺭﻳﺭ ‪:‬‬
‫‪ .١‬ﻣﻛﻭﻧﺎﺕ ﺍﻟﺧﻠﻁﻪ ﺍﻻﺳﻔﻠﺗﻳﺔ‪ ،‬ﺍﻟﻣﺻﺩﺭ‪.‬‬
‫‪ .٢‬ﻋﺩﺩ ﺍﻟﻁﺭﻗﺎﺕ ﻋﻠﻲ ﻛﻝ ﺟﻬﻪ ﻟﻠﻌﻳﻧﺔ‪.‬‬
‫ﺗﺟﺭﺑﻪ ﺭﻗﻡ ‪  -١٣-‬‬
‫ﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ ﺍﻟﻛﻠﻲ ﻟﺧﻠﻁﺔ ﺍﺳﻔﻠﺗﻳﻪ ﻣﺩﻣﻭﻛﻪ‬
‫‪  Bulk Specific Gravity of Compacted Bituminous Mixtures ‬‬
‫‪  ASTM D2726‬‬
‫‪ ‬ﺍﻟﻐﺭﺽ ‪:‬‬
‫ﻟﺣﺳﺎﺏ ﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ ﺍﻟﻛﻠﻲ )‪ (Bulk Specific Gravity‬ﻟﻌﻳﻧﺔ ﺍﺳﻔﻠﺕ ﻣﺩﻣﻭﻛﺔ‪.‬‬
‫‪ ‬ﺍﻻﻫﻣﻳﺔ ﻭﺍﻻﺳﺗﺧﺩﺍﻡ ‪:‬‬
‫ﻧﺗﺎﺋﺞ ﻫﺫﺍ ﺍﻻﺧﺗﺑﺎﺭ ﺗﺳﺗﺧﺩﻡ ﻟﺗﺣﻠﻳﻝ ﺍﻟﻔﺭﻏﺎﺕ ﻟﺧﻠﻳﻁ ﺍﻻﺳﻔﻠﺕ ﺍﻟﻣﺩﻣﻭﻙ‪.‬‬
‫‪ ‬ﻋﻳﻧﺔ ﺍﻻﺧﺗﺑﺎﺭ ‪:‬‬
‫ﺧﻠﻁﻪ ﺍﺳﻔﻠﺗﻳﻪ ﻣﻌﺩﻩ ﺑﺎﺳﺗﺧﺩﺍﻡ ﻣﺎﺭﺷﺎﻝ ﺍﻭ ﻗﻭﺍﻟﺏ ﻣﻥ ﺍﻟﺭﺻﻑ ﺍﻻﺳﻔﻠﺗﻲ‪.‬‬
‫‪ ‬ﺍﻻﺟﻬﺯﺓ ‪:‬‬
‫‪ .١‬ﻣﻳﺯﺍﻥ‪.‬‬
‫‪ .٢‬ﺣﻣﺎﻡ ﻣﺎﺋﻲ‪.‬‬
‫ﺧﻁﻭﺍﺕ ﺍﻻﺧﺗﺑﺎﺭ ‪:‬‬ ‫‪‬‬
‫ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ ﻓﻲ ﺍﻟﻬﻭﺍء ﻭﻟﻳﻛﻥ )‪.(A‬‬ ‫‪.١‬‬
‫ﻏﻣﺭ ﺍﻟﻌﻳﻧﻪ ﻓﻲ ﺍﻟﻣﻳﺎﻩ ﻋﻧﺩ ﺩﺭﺟﻪ ﺣﺭﺍﺭﻩ )‪ (١ ± ٢٥‬ﺩﺭﺟﻪ ﻣﺋﻭﻳﻪ ﻟﻣﺩﻩ ﺗﺗﺭﺍﻭﺡ ﻣﻥ )‪٣‬‬ ‫‪.٢‬‬
‫‪ (٥ :‬ﺩﻗﺎﺋﻖ ﻭﻟﻳﻛﻥ ﻭﺯﻧﻬﺎ ﻓﻲ ﺍﻟﻣﻳﺎﻩ )‪ (C‬ﺷﻛﻝ )‪.(١-١١‬‬
‫ﺇﺯﺍﻟﻪ ﺍﻟﻌﻳﻧﺔ ﻣﻥ ﺍﻟﻣﻳﺎﻩ‪ ،‬ﻭﺗﺟﻔﻳﻑ ﺍﻟﺳﻁﺢ ﺑﺎﺳﺗﺧﺩﺍﻡ ﻗﻁﻌﻪ ﻗﻣ ﺎﺵ ﺭﻁﺑ ﺔ‪ ،‬ﻭﺣﺳ ﺎﺏ ﻭﺯﻥ‬ ‫‪.٣‬‬
‫ﺍﻟﻌﻳﻧﺔ ﻣﺷﺑﻌﻪ ﺟﺎﻓﺔ ﺍﻟﺳﻁﺢ ﻭﻟﻳﻛﻥ )‪  .(B‬‬

‫ﺷﻛﻝ )‪ (١-١٣‬ﺗﻌﻳﻥ ﻭﺯﻥ ﺍﻟﻌﻳﻧﻪ ﻓﻲ ﺍﻟﻣﺎء‬ ‫‪ ‬ﺍﻟﺗﺣﻠﻳﻝ ﻭﺍﻟﻧﺗﺎﺋﺞ ‪:‬‬


‫ﺣﺳﺎﺏ ﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ ﺍﻟﻛﻠﻲ ‪:‬‬

‫ﺣﻳﺙ ‪:‬‬
‫‪ :A‬ﻭﺯﻥ ﺍﻟﻌﻳﻧﻪ ﻓﻲ ﺍﻟﻬﻭﺍء‪ ،‬ﺟﻡ‪.‬‬
‫‪ :B‬ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ ﻣﺷﺑﻌﻪ ﺟﺎﻓﻪ ﺍﻟﺳﻁﺢ‪ ،‬ﺟﻡ‪.‬‬
‫‪ :C‬ﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ ﻓﻲ ﺍﻟﻣﺎء‪ ،‬ﺟﻡ‪.‬‬
‫‪ ‬ﺍﻟﺗﻘﺭﻳﺭ ‪:‬‬
‫ﻗﻳﻣﻪ ﺍﻟﻭﺯﻥ ﺍﻟﻧﻭﻋﻲ ﺍﻟﻛﻠﻲ ﻻﻗﺭﺏ ‪ ٣‬ﻋﻼﻣﺎﺕ ﻋﺷﺭﻳﻪ‪.‬‬
‫ﺗﺟﺭﺑﻪ ﺭﻗﻡ ‪  -١٤-‬‬
‫ﺛﺑﺎﺕ ﻣﺎﺭﺷﺎﻝ ﻭﺍﻻﻧﻔﻌﺎﻝ ﻟﻠﺧﻠﻁﺎﺕ ﺍﻻﺳﻔﻠﺗﻳﺔ‬
‫‪  Marshall Stability and flow of Asphalt Concrete‬‬
‫‪  ASTM D1559‬‬
‫‪ ‬ﺍﻟﻐﺭﺽ ‪:‬‬
‫ﺣﺳﺎﺏ ﻗﻳﻣﻪ ﺛﺑﺎﺕ ﻣﺎﺭﺷﺎﻝ ﻭﺍﻻﻧﻔﻌﺎﻝ ﻟﻠﺧﻠﻁﺎﺕ ﺍﻻﺳﻔﻠﺗﻳﺔ‪.‬‬
‫‪ ‬ﺍﻻﻫﻣﻳﺔ ﻭﺍﻻﺳﺗﺧﺩﺍﻡ ‪  :‬‬
‫ﻟﻣﻌﺭﻓﻪ ﺧﺻﺎﺋﺹ ﺍﻟﺧﻠﻁﻪ ﺍﻻﺳﻔﻠﺗﻳﻪ‬
‫ﺍﻻﺟﻬﺯﻩ ‪:‬‬ ‫‪‬‬
‫ﺟﻬﺎﺯ ﻣﺎﺭﺷﺎﻝ‪) .‬ﻳﺗﺣﺭﻙ ﺑﺎﻧﺗﻅﺎﻡ ﺭﺍﺳﻳﺎ ﺑﻣﻌﺩﻝ ‪ ٥٠٫٨‬ﻣﻡ‪/‬ﺩﻗﻳﻘﻪ(‪.‬‬ ‫‪.١‬‬
‫ﺣﻣﺎﻡ ﻣﺎﺋﻲ‪.‬‬ ‫‪.٢‬‬
‫ﺟﻬﺎﺯ ﻟﻘﻳﺎﺱ ﺍﻟﺣﻣﻝ‪ ،‬ﻭﺟﻬﺎﺯ ﻟﻘﻳﺎﺱ ﺍﻻﻧﻔﻌﺎﻝ‪.‬‬ ‫‪.٣‬‬
‫ﺧﻁﻭﺍﺕ ﺍﻟﺗﺟﺭﺑﺔ ‪:‬‬ ‫‪‬‬
‫ﻭﺿ ﻊ ﺍﻟﻌﻳﻧ ﺔ ﻑ ﺣﻣ ﺎﻡ ﻣ ﺎﺋﻲ ﻋﻧ ﺩﺭ ﺩﺭﺟ ﻪ ﺣ ﺭﺍﺭﻩ ‪ ٦٠‬ﺩﺭﺟ ﺔ ﻣﺋﻭﻳ ﻪ ﻟﻣ ﺩﻩ‬ ‫‪.١‬‬
‫)‪ (٤٠ : ٣٠‬ﺩﻗﻳﻘﻪ ﺍﻭ ﺗﻭﺿﻊ ﻓﻲ ﺍﻟﻔﺭﻥ ﻟﻣﺩﻩ ﺳﺎﻋﺗﻳﻥ‪.‬‬
‫ﺇﺯﺍﻟﻪ ﺍﻟﻌﻳﻧﺔ ﻣﻥ ﺍﻟﺣﻣﺎﻡ ﺍﻟﻣﺎﺋﻲ ﻭﻭﺿﻌﻬﺎ ﻓﻲ ﺟﻬﺎﺯ ﻣﺎﺭﺷﺎﻟﺷﻛﻝ )(‪.‬‬ ‫‪.٢‬‬
‫ﺗﻌ ﺭﻳﺽ ﺍﻟﻌﻳﻧ ﺔ ﻟﺣﻣ ﻝ ﺑﻣﻌ ﺩﻝ ﺛﺎﺑ ﺕ )‪ ٥٠٫٨‬ﻣﻡ‪/‬ﺩﻗﻳﻘ ﻪ( ﺣﺗ ﻲ ﺍﻟﻭﺻ ﻭﻝ‬ ‫‪.٣‬‬
‫ﻻﻗﺻﻲ ﺣﻣﻝ ﻭﺣﺗﻲ ﻳﻘﻝ ﺍﻟﺣﻣﻝ‪ .‬ﺯﻣﻥ ﺍﺟﺭﺍء ﺍﻻﺧﺗﺑﺎﺭ ﻣﻥ ﺍﺯﺍﻟﻪ ﺍﻟﻌﻳﻧﻪ ﻣﻥ‬
‫ﺍﻟﺣﻣﺎﻡ ﺍﻟﻣﺎﺋﻲ ﺍﻭ ﺍﻟﻔﺭﻥ ﻭﺣﺗﻲ ﺣﻣﻝ ﺍﻟﻛﺳﺭ ﻻﺗﺯﻳﺩ ﻋﻥ ‪ ٣٠‬ﺛﺎﻧﻳﻪ‪.‬‬
‫ﻳ ﺗﻡ ﻗ ﺭﺍءﻩ ﻗﻳﻣ ﻪ ﺛﺑ ﺎﺕ ﻣﺎﺭﺷ ﺎﻝ )ﺣﻣ ﻝ ﺍﻟﻛﺳ ﺭ( ﻭﺍﻻﻧﻔﻌ ﺎﻝ )ﺍﻟﺗﻐﻳ ﺭ ﺍﻟﺣ ﺎﺩﺙ‬ ‫‪.٤‬‬
‫ﻋﻧﺩ ﺣﻣﻝ ﺍﻟﻛﺳﺭ(‪.‬‬
‫ﺍﺫﺍ ﻛﺎﻥ ﺍﺭﺗﻔﺎﻉ ﺍﻟﻌﻳﻧﻪ ﻻﻳﺳ ﺎﻭﻱ‬ ‫‪.٥‬‬
‫ﺷﻛﻝ )‪ (١-١٤‬ﺟﻬﺎﺯ ﻣﺎﺭﺷﺎﻝ‬ ‫ﺎﺕ‬ ‫‪ ٦٣٬٥‬ﻣ ﻡ‪ ،‬ﺗﺿ ﺭﺏ ﻳﻣ ﻪ ﺛﺑ‬
‫)ﺟﺩﻭﻝ ‪  .(١‬‬ ‫ﻣﺎﺭﺷ ﺎﻝ ﻓ ﻲ ﻣﻌﺎﻣ ﻝ ﺗﺻ ﺣﻳﺢ‬
‫‪ ‬‬

‫‪ ‬ﻣﻌﺎﻣﻼﻟﺗﺻﺣﻳﺢ‬ ‫‪ ‬ﺳﻣﻛﺎﻟﻌﻳﻧﻪ )ﻣﻡ(‬ ‫ﻣﻌﺎﻣﻝ ﺍﻟﺗﺻﺣﻳﺢ‬ ‫ﺳﻣﻙ ﺍﻟﻌﻳﻧﻪ )ﻣﻡ(‬


‫‪٠٬٩٦‬‬ ‫‪٦٥٬١‬‬ ‫‪١٬٤٧‬‬ ‫‪٥٠٬٨‬‬
‫‪٠٬٩٣‬‬ ‫‪٦٦٬٧‬‬ ‫‪١٬٣٩‬‬ ‫‪٥٢٬٤‬‬
‫‪٠٬٨٩‬‬ ‫‪٦٨٬٣‬‬ ‫‪١٬٣٢‬‬ ‫‪٥٤‬‬
‫‪٠٬٨٦‬‬ ‫‪٦٩٬٨‬‬ ‫‪  ١٬٢٥‬‬ ‫‪٥٥٬٦‬‬
‫‪٠٬٨٣‬‬ ‫‪٧١٬٤‬‬ ‫‪١٬١٩‬‬ ‫‪٥٧٬٢‬‬
‫‪٠٬٨١‬‬ ‫‪٧٣٬٠٠‬‬ ‫‪١٬١٤‬‬ ‫‪٥٨٬٧‬‬
‫‪٠٬٧٨‬‬ ‫‪٧٤٬٦‬‬ ‫‪١٬٠٩‬‬ ‫‪٦٠٬٣‬‬
‫‪٠٬٧٦‬‬ ‫‪٧٦٬٢‬‬ ‫‪١٬٠٤‬‬ ‫‪٦١٬٩‬‬
‫‪  ١٬٠٠‬‬ ‫‪٦٣٬٥‬‬

‫‪ ‬‬
‫‪ ‬ﺍﻟﻧﺗﺎﺋﺞ ‪  :‬‬
‫ﺗﻭﻗﻳﻊ ﺍﻟﻣﻧﺣﻧﻳﺎﺕ ﺍﻟﺗﻲ ﺗﺭﺑﻁ ﻧﺳﺑﻪ ﺍﻻﺳﻔﻠﺕ ﺍﻟﻣﺧﺗﻠﻔﻪ ﻣﻊ ‪:‬‬
‫‪ .١‬ﻣﻘﺩﺍﺭ ﺍﻻﺳﻔﻠﺕ ﺑﺎﻟﺭﻁﻝ‪.‬‬
‫‪٣‬‬
‫‪ .٢‬ﻭﺯﻥ ﻭﺣﺩﻩ ﺍﻟﺣﺟﻭﻡ‪ ،‬ﻁﻥ‪/‬ﻡ‬
‫‪ .٣‬ﻧﺳﺑﻪ ﺍﻟﻔﺭﺍﻏﺎﺕ ﺍﻟﻛﻠﻳﻪ ﺑﺎﻟﻣﺧﻠﻭﻁ ﺍﻻﺳﻔﻠﺗﻲ )‪.(%‬‬
‫‪ .٤‬ﻧﺳﺑﻪ ﺍﻟﻔﺭﺍﻏﺎﺕ ﺑﺎﻟﻣﻭﺍﺩ ﺍﻟﺻﻠﺑﻪ )‪.(%‬‬
‫‪ .٥‬ﻣﻘﺩﺍﺭﺍﻹﻧﺳﻳﺎﺏ )‪ ١٠٠/١‬ﻣﻥ ﺍﻟﺑﻭﺻﻪ(‪  .‬‬

‫ﺷﻛﻝ‬

‫)‪ (٢-١٤‬ﺍﻟﻣﻧﺣﻧﻳﺎﺕ ﺍﻟﺗﺻﻣﻳﻣﻪ ﻟﻠﺧﻠﻁﺎﺕ ﺍﻻﺳﻔﻠﺗﻳﻪ‬


‫ﺍﻟﺗﻘﺭﻳﺭ ‪:‬‬ ‫‪‬‬
‫ﻧﻭﻉ ﺍﻟﻌﻳﻧﻪ )ﺗﺟﻬﻳﺯ ﻣﻌﻣﻝ ﺍﻭ ﻗﺎﻟﺏ(‬ ‫‪.١‬‬
‫ﻣﺗﻭﺳﻁ ﺛﺑﺎﺕ ﻣﺎﺭﺷﺎﻝ ﻣﺻﺣﺢ ﻟﺛﻼﺙ ﻋﻳﻧﺎﺕ ﻣﺗﻣﺎﺛﻠﻪ )ﻣﻌﺩﻩ ﺑﻧﻔﺱ ﻣﺣﺗﻭﻱ ﺍﻻﺳﻔﻠﺕ(‪.‬‬ ‫‪.٢‬‬
‫ﻣﺗﻭﺳﻁ ﺍﻧﻔﻌﺎﻝ ﻣﺎﺭﺷﺎﻝ ﻟﺛﻼﺙ ﻋﻳﻧﺎﺕ ﻣﺗﻣﺎﺛﻠﻪ )ﻣﻌﺩﻩ ﺑﻧﻔﺱ ﻣﺣﺗﻭﻱ ﺍﻻﺳﻔﻠﺕ(‪  .‬‬ ‫‪.٣‬‬
‫ﺗﻌﻳﻳﻥ ﻣﺣﺗﻭﻱ ﺍﻻﺳﻔﻠﺕ ﺍﻟﺫﻱ ﻳﺣﻘﻖ ﺍﻋﻠﻲ ﺛﺑﺎﺕ )‪  .(A‬‬ ‫‪.٤‬‬
‫ﺗﻌﻳﻳﻥ ﻣﺣﺗﻭﻱ ﺍﻻﺳﻔﻠﺕ ﺍﻟﺫﻱ ﻳﺣﻘﻖ ﻧﺳﺑﻪ ﻓﺭﺍﻏﺎﺕ ﻫﻭﺍﺋﻳﻪ )‪  .(B) %(٥ : ٣‬‬ ‫‪.٥‬‬
‫ﺗﻌﻳﻳﻥ ﻣﺣﺗﻭﻱ ﺍﻻﺳﻔﻠﺕ ﺍﻟﺫﻱ ﻳﺣﻘﻖ ﺍﻋﻠﻲ ﻛﺛﺎﻓﺔ ﻧﺳﺑﻳﻪ ﻗﺻﻭﻱ )‪  .(C‬‬ ‫‪.٦‬‬
‫ﺣﺳﺎﺏ ﺍﻟﻣﺣﺗﻭﻱ ﺍﻻﺳﻔﻠﺗﻲ ﺍﻻﻣﺛﻝ )‪  .(Optimum Asphalt Content‬‬ ‫‪.٧‬‬
‫ﺍﻟﺗﺎﻛ ﺩ ﻣ ﻥ ﻣﻁﺎﺑﻘ ﻪ ﻗ ﻳﻡ ﺍﻝ )‪ (VMA & Air Voids &  Stability & Flow &  VFA‬ﺍﻟﻣﻘﺎﺑﻠ ﻪ ﻟﻠﻣﺣﺗ ﻭﻱ ﺍﻻﺳ ﻔﻠﺗﻲ ﺍﻻﻣﺛ ﻝ‬ ‫‪.٨‬‬
‫ﻟﻠﻣﻭﺍﺻﻔﺎﺕ‪  .‬‬
‫‪ ‬‬
‫ﺗﺟﺭﺑﻪ ﺭﻗﻡ ‪  -١٥-‬‬
‫ﺍﻻﺧﺗﺑﺎﺭ ﺍﻟﻘﻳﺎﺳﻲ ﻻﺳﺗﺧﻼﺹ ﺍﻻﺳﻔﻠﺕ ﻣﻥ ﺧﻠﻁﺎﺕ ﺍﻟﺭﺻﻑ ﺍﻻﺳﻔﻠﺗﻳﻪ‬
‫‪  Quantitative Extraction of Bitumen from Bituminous Paving Mixtures‬‬
‫‪  ASTM D2172‬‬
‫‪ ‬ﺍﻟﻐﺭﺽ ‪:‬‬
‫ﻳﺳﺗﺧﺩﻡ ﻫﺫﺍ ﺍﻻﺧﺗﺑﺎﺭ ﻟﺣﺳﺎﺏ ﻛﻣﻳﻪ ﺍﻟﺑﻳﺗﻭﻣﻳﻥ ﻓﻲ ﺧﻠﻁﺎﺕ ﺍﻟﺭﺻﻑ ﺍﻻﺳﻔﻠﺗﻳﻪ ﺍﻟﺳﺎﺧﻧﻪ ﻭﻋﻳﻧ ﺎﺕ ﺍﻻﺳ ﻔﻠﺕ‪ .‬ﺍﻟﺭﻛ ﺎﻡ ﺍﻟﻣﺳ ﺗﺧﻠﺹ‬
‫ﻣﻥ ﻫﺫﺍ ﺍﻻﺧﺗﺑﺎﺭ ﻳﻣﻛﻥ ﺍﺳﺗﺧﺩﺍﻣﻪ ﻓﻲ ﺍﺧﺗﺑﺎﺭ ﺍﻟﺗﺣﻠﻳﻝ ﺍﻟﻣﻧﺧﻠﻲ‪.‬‬
‫‪ ‬ﺍﻻﻫﻣﻳﺔ ﻭﺍﻻﺳﺗﺧﺩﺍﻡ ‪  :‬‬
‫ﻳﺳﺗﺧﺩﻡ ﻫﺫﺍ ﺍﻻﺧﺗﺑﺎﺭ ﻟﺣﺳﺎﺏ ﻛﻳﻣﻪ ﺍﻟﺑﻳﺗﻭﻣﻳﻥ ﻓﻲ ﺧﻠﻁﺎﺕ ﺍﻟﺭﺻﻑ ﺍﻻﺳﻔﻠﺗﻳﻪ ﻭﻋﻳﻧﺎﺕ ﺍﻻﺳﻔﻠﺕ ﻟﻘﺑﻭﻝ ﺍﻟﻣﻭﺍﺻﻔﻪ ﻭﺍﻟﺗﻘﻳﻳﻡ‪  .‬‬
‫‪ ‬ﺍﻻﺟﻬﺯﻩ ‪:‬‬
‫ﻓﺭﻥ‪ ،‬ﻗﺎﺩﺭ ﻋﻠﻲ ﺍﻟﺣﻔﺎﻅ ﻋﻠﻲ ﺩﺭﺟﻪ ﺍﻟﺣﺭﺍﺭﻩ ﻋﻧﺩ )‪ (٥ ± ١١٠‬ﺩﺭﺟﻪ ﻣﺋﻭﻳﻪ‪.‬‬
‫ﻭﻋﺎء ﻣﺳﻁﺢ‪.‬‬
‫ﻣﻳﺯﺍﻥ ﺫﻭ ﺩﻗﻪ ﻻ ﺗﻘﻝ ﻋﻥ ‪ %٠٫٠١‬ﻣﻥ ﻭﺯﻥ ﺍﻟﻌﻳﻧﻪ‪.‬‬
‫ﺳﺧﺎﻥ ﻛﻬﺭﺑﻲ‪ ،‬ﺫﻭ ﻗﺩﺭﻩ ﻛﻬﺭﺑﻳﻪ ﻣﺗﻐﻳﺭﻩ‪.‬‬
‫ﻭﻋﺎء ﺫﻭ ﻓﺗﺣﻪ ﻋﻠﻳﺎ ﺻﻐﻳﺭﻩ‪.‬‬
‫ﻭﻋﺎء ﺍﺷﺗﻌﺎﻝ ﺳﻌﺗﻪ‪.‬‬
‫ﻭﻋﺎء ﺗﺟﻔﻳﻑ‪.‬‬
‫ﺣﻠﻘﻪ ﺗﺭﺷﻳﺢ‪ ،‬ﻭﺭﻗﻳﻪ‪.‬‬
‫ﺟﻬﺎﺯ ﺍﻻﺳﺗﺧﻼﺹ‪ ،‬ﻳﺗﻛﻭﻥ ﻣﻥ ﺣﻠﻪ ﻣﻭﺿﺣﻪ ﻓﻲ ﺍﻟﺷﻛﻝ )‪ ،(١-١٥‬ﻭﺟﻬﺎﺯ ﻟﺗ ﺩﻭﻳﺭ ﺍﻟﺣﻠ ﻪ ﺑﺳ ﺭﻋﺎﺕ ﻣﺗﻐﻳ ﺭﻩ ﻳﻣﻛ ﻥ ﺍﻟ ﺗﺣﻛﻡ‬
‫ﺑﻪ ﺗﺻﻝ ﻟـ ‪ ٣٦٠٠‬ﻟﻔﻪ ﻓﻲ ﺍﻟﺩﻗﻳﻘﻪ‪ .‬ﻳﻣﻛﻥ ﺍﻟﺗﺣﻛﻡ ﻓﻲ ﺍﻟﺳﺭﻋﻪ ﻳﺩﻭﻳﺎ ﺍﻭ ﺑﺿﺑﻁ ﺍﻟﺳﺭﻋﻪ ﻣﺳﺑﻘﺎ‪ .‬ﻳﻧﺑﻘﻲ ﺗﺯﻭﻳ ﺩ ﺍﻟﺟﻬ ﺎﺯ ﺑﻭﻋ ﺎء‬
‫ﻟﺗﺟﻣﻳﻊ ﺍﻟﻣﺫﻳﺏ ﺍﻟﻣﻠﻘﻲ ﻣﻥ ﺍﻟﺣﻠﻪ ﻭ ﺣﻧﻔﻳﻪ ﺍﻟﺻﺭﻑ ﻻﺯﺍﻟﻪ ﺍﻟﻣﺫﻳﺏ‪.‬‬

‫ﺷﻛﻝ‪ ٢-١٥‬ﺟﻬﺎﺯ ﺍﻻﺳﺗﺧﻼﺹ‬

‫ﺭﺳﻣﺗﻭﺿﻳﺣﻲ‪ ١-١٥‬ﺣﻠﻪ ﺍﻻﺳﺗﺧﻼﺹ‬


‫‪ ‬‬ ‫‪ ‬‬
‫ﺧﻁﻭﺍﺕ ﺍﻟﺗﺟﺭﺑﺔ ‪:‬‬

‫ﺗﺳﺧﻳﻥ ﺍﻟﻌﻳﻧﻪ ﺍﻻﺳﻔﻠﺗﻳﻪ ﻓﻲ ﺍﻟﻔﺭﻥ ﻋﻧﺩ ﺩﺭﺟﻪ ﺣﺭﺍﺭﻩ ‪ ٦٠‬ﺩﺭﺟﻪ ﻣﺋﻭﻳﻪ ﻟﻠﺗﺟﻔﻳﻑ‪.‬‬ ‫‪.١‬‬
‫ﻭﺿﻊ )‪ (٢٥٠٠ : ٧٥٠‬ﺟﻡ ﻣﻥ ﻋﻳﻧﻪ ﺍﻻﺧﺗﺑﺎﺭ ﺍﻟﻣﺟﻔﻔﻪ ﺳﺎﺑﻘﺎ ﻟﻭﺯﻥ ﺛﺎﺑﺕ ﻣﻊ ﺣﻠﻘﻪ ﺍﻟﺗﺭﺷﻳﺢ ﻓﻲ ﺍﻟﺣﻠﻪ‪.‬‬ ‫‪.٢‬‬
‫ﺗﻐﻁﻳﻪ ﺍﻟﻌﻳﻧﻪ ﻓ ﻲ ﺍﻟﺣﻠ ﻪ ﺏ ﺛﻼﺛ ﻲ ﻛﻠ ﻭﺭﺍﻻﻳﺛﻳﻠﻳﻥ‪ ،‬ﺑﺭﻭﻣﻳ ﺩ ﺑﺭﻭﺑﻳ ﻝ ﻋ ﺎﺩﻱ ﺍﻭ ﻛﻠﻭﺭﻳ ﺩ ﺍﻟﻣﻳﺛﻳﻠ ﻳﻥ‪ .‬ﺗ ﺭﻙ ﺍﻟﻌﻳﻧ ﻪ ﻟﻭﻗ ﺕ‬ ‫‪.٣‬‬
‫ﻛ ﺎﻓﻲ ﺣﺗ ﻲ ﻳﺣﻠ ﻝ ﺍﻟﻣ ﺫﻳﺏ ﺍﻟﻌﻳﻧ ﻪ )ﻻﻳﺯﻳ ﺩ ﻋ ﻥ ‪ ١‬ﺳﺎﻋﻪ(‪.‬ﻭﺿ ﻊ ﺍﻟﺣﻠ ﻪ ﺍﻟﻣﺣﺗ ﻭﺍﻩ ﻋﻠ ﻲ ﺍﻟﻌﻳﻧ ﻪ ﻭﺍﻟﻣ ﺫﻳﺏ ﻓ ﻲ ﺟﻬ ﺎﺯ‬
‫ﺍﻻﺳﺗﺧﻼﺹ‪ .‬ﺗﺟﻔﻳﻑ ﻭﺣﺳﺎﺏ ﻭﺯﻥ ﺣﻠﻘﻪ ﺍﻟﺗﺭﺷﻳﺢ ﻭﻭﺿﻌﻬﺎ ﻋﻠﻲ ﺣﻭﺍﻑ ﺍﻟﺣﻠﻪ‪ .‬ﺗﺛﺑﻳﺕ ﺍﻟﻐﻁﺎء ﻋﻠ ﻲ ﺍﻟﺣﻠ ﻪ ﺑﺈﺣﻛ ﺎﻡ‬
‫ﻭﻭﺿﻊ ﺍﻟﻭﻋﺎء ﺍﺳﻔﻝ ﺍﻟﺣﻧﻔﻳﻪ ﻟﺗﺟﻣﻳﻊ ﺍﻟﻣﺫﻳﺏ ﻭﺍﻟﺑﻳﺗﻭﻣﻳﻥ ﺍﻟﻣﺳﺗﺧﻠﺹ‪.‬‬
‫ﺗﺷ ﻐﻳﻝ ﺟﻬ ﺎﺯ ﺍﻟﻁ ﺭﺩ ﺍﻟﻣﺭﻛ ﺯﻱ ﺑ ﺑﻁء‪ ،‬ﺯﻳ ﺎﺩﻩ ﺳ ﺭﻋﻪ ﺍﻟ ﺩﻭﺭﺍﻥ ﺗ ﺩﺭﻳﺟﻳﺎ ﺣﺗ ﻲ ﺗﺻ ﻝ ﺍﻟﺳ ﺭﻋﻪ ﺍﻟ ﻲ ﺍﻟﺣ ﺩ ﺍﻻﻗﺻ ﻲ‬ ‫‪.٤‬‬
‫‪ ٣٦٠٠‬ﻟﻔﻪ ﻓﻲ ﺍﻟﺩﻗﻳﻘﻪ ﺍﻭ ﺣﺗﻲ ﻳﺗﻭﻗﻑ ﺍﻟﻣﺫﻳﺏ ﻣﻥ ﺍﻟﺗ ﺩﻓﻖ ﻣ ﻥ ﺣﻧﻔﻳ ﻪ ﺍﻟﺻ ﺭﻑ‪ .‬ﺍﻳﻘ ﺎﻑ ﺍﻟﺟﻬ ﺎﺯ‪ ،‬ﺍﺿ ﺎﻓﻪ ‪ ٢٠٠‬ﻣﻠ ﻲ‬
‫ﻣﻥ ﺛﻼﺛﻲ ﻛﻠﻭﺭ ﺍﻻﻳﺛﻳﻠﻳﻥ‪ ،‬ﺑﺭﻭﻣﻳﺩ ﺑﺭﻭﺑﻳﻝ ﻋﺎﺩﻱ ﺍﻭ ﻛﻠﻭﺭﻳﺩ ﺍﻟﻣﻳﺛﻳﻠ ﻳﻥ ﻭﺗﻛ ﺭﺍﺭ ﺍﻟﺧﻁ ﻭﺗﻳﻥ ﺍﻟﺳ ﺎﺑﻘﺗﻳﻥ‪ .‬ﺍﺿ ﺎﻓﻪ ‪٢٠٠‬‬
‫ﻣﻠﻲ ﻣﻥ ﺍﻟﻣﺫﻳﺏ ﻋﻠﻲ ﺍﻻﻗﻝ ﺛﻼﺙ ﻣﺭﺍﺕ ﺣﺗﻲ ﻳﺻﻝ ﻟﻭﻥ ﺍﻟﻣﺫﻳﺏ ﺍﻟﻣﺳﺗﺧﻠﺹ ﻟﻠﻭﻧﻪ ﺍﻟﻁﺑﻳﻌﻲ )ﺍﺻ ﻔﺭ ﺷ ﺎﺣﺏ(‪ .‬ﻳ ﺗﻡ‬
‫ﺗﺟﻣﻳﻊ ﻧﺎﺗﺞ ﺍﻻﺳﺗﺧﻼﺹ ﻓﻲ ﻭﻋﺎء ﻣﻧﺎﺳﺏ‪  .‬‬
‫ﺇﺯﺍﻟﻪ ﺣﻠﻘﻪ ﺍﻟﺗﺭﺷﻳﺢ ﻣﻥ ﺍﻟﺣﻠﻪ ﻭﺗﺟﻔﻳﻔﻬﺎ ﻓﻲ ﺍﻟﻬﻭﺍء‪ .‬ﻓﻲ ﺣﺎﻟﻪ ﺍﺳﺗﺧﺩﺍﻡ ﺣﻠﻘﻪ ﺗﺭﺷﻳﺢ ﻣﺻﻧﻭﻋﻪ ﻣﻥ ﺍﻟﻠﺑﺎﺩ‪ ،‬ﻳﺗﻡ ﺗﻧﻅﻳﻑ‬ ‫‪.٥‬‬
‫ﺳﻁﺢ ﺣﻠﻘﻪ ﺍﻟﺗﺭﺷ ﻳﺢ ﺑﺎﻟﻔﺭﺷ ﺎﻩ ﻣ ﻥ ﺍﻟﻣ ﻭﺍﺩ ﺍﻟﻧﺎﻋﻣ ﻪ ﺍﻟﻣﻠﺗﺻ ﻘﻪ ﺑﺣﻠﻘ ﻪ ﺍﻟﺗﺭﺷ ﻳﺢ ﻭﺇﺿ ﺎﻓﺗﻬﺎ ﻋﻠ ﻲ ﺍﻟﺭﻛ ﺎﻡ ﺍﻟﻣﺳ ﺗﺧﻠﺹ‪.‬‬
‫ﺗﺟﻔﻳﻑ ﺣﻠﻘﻪ ﺍﻟﺗﺭﺷﻳﺢ ﻟﻭﺯﻥ ﺛﺎﺑﺕ ﻓﻲ ﺍﻟﻔﺭﻥ ﻋﻧ ﺩ )‪ (٥ ± ١١٠‬ﺩﺭﺟ ﻪ ﻣﺋﻭﻳ ﻪ‪ .‬ﺇﺯﺍﻟ ﻪ ﻛ ﻝ ﻣﺣﺗﻭﻳ ﺎﺕ ﺍﻟﺣﻠ ﻪ ﺑﺣ ﺭﺹ‬
‫ﻓﻲ ﻭﻋﺎء ﺻﻠﺏ ﻭﺗﺟﻔﻳﻔﻪ ﻓﻲ ﺣﻣﺎﻡ ﺑﺧﺎﺭ‪ ،‬ﻭﺗﺟﻔﻳﻔﻬﺎ ﻟﻭﺯﻥ ﺛﺎﺑﺕ ﻓﻲ ﺍﻟﻔﺭﻥ ﺍﻭ ﻋﻠﻲ ﺳﺧﺎﻥ ﻋﻧ ﺩ )‪ (٥ ± ١١٠‬ﺩﺭﺟ ﻪ‬
‫ﻣﺋﻭﻳﻪ‪ .‬ﻓﻲ ﺣﺎﻟﻪ ﺍﺳﺗﺧﺩﺍﻡ ﺛﻼﺛﻲ ﻛﻠﻭﺭﻳﺩ ﺍﻻﻳﺛﻠ ﻳﻥ‪ ،‬ﺑﺭﻭﻣﻳ ﺩ ﺑﺭﻭﺑﻳ ﻝ ﻋ ﺎﺩﻱ ﺍﻭ ﻛﻣ ﺫﻳﺏ ﺍﺳ ﺗﺧﻼﺹ‪ ،‬ﻳﻣﻛ ﻥ ﺍﻻﺳ ﺗﻐﻧﺎء‬
‫ﻋ ﻥ ﺗﺟﻔﻳ ﻑ ﺍﻟﻌﻳﻧ ﻪ ﺍﻟﻣﺑ ﺩﺋﻲ ﻓ ﻲ ﺣﻣ ﺎﻡ ﺍﻟﺑﺧ ﺎﺭ ﻭﺯﻥ ﺍﻟﺭﻛ ﺎﻡ ﺍﻟﻣﺳ ﺗﺧﻠﺹ )ﻭ‪ (٢‬ﻳﺳ ﺎﻭﻱ ﻭﺯﻥ ﺍﻟﺭﻛ ﺎﻡ ﻓ ﻲ ﺍﻟﻭﻋ ﺎء‬
‫ﺑﺎﻻﺿﺎﻓﻪ ﺍﻟﻲ ﺍﻟﺯﻳﺎﺩﻩ ﻓﻲ ﺍﻟﻭﺯﻥ ﻣﻥ ﺣﻠﻘﺎﺕ ﺍﻟﺗﺭﺷﻳﺢ‪  .‬‬
‫ﻓﻲ ﺣﺎﻟﻪ ﺍﺳﺗﺧﺩﺍﻡ ﻭﺭﻗﻪ ﺗﺭﺷ ﻳﺢ ﻣﻧﺧﻔﺿ ﻪ ﺍﻟﺭﻣ ﺎﺩ ﻳ ﺗﻡ ﺍﺟ ﺭﺍء ﺍﻟﺧﻁ ﻭﻩ ﺍﻻﺗﻳ ﻪ‪ :‬ﻭﺿ ﻊ ﺍﻟﺭﻛ ﺎﻡ ﻭﺣﻠﻘ ﺎﺕ ﺍﻟﺗﺭﺷ ﻳﺢ ﻓ ﻲ‬ ‫‪.٦‬‬
‫ﻭﻋﺎء ﻣﻌﺩﻧﻲ ﻧﻅﻳﻑ‪ .‬ﻭﺗﺟﻔﻳﻑ ﺍﻟﻌﻳﻧﻪ ﻛﻣﺎ ﺳﺑﻖ ﺗﻭﺿﻳﺣﻬﺎ‪ .‬ﺛﻧﻲ ﺣﻠﻘﻪ ﺍﻟﺗﺭﺷﻳﺢ ﺍﻟﺟﺎﻓﻪ ﻭﻭﺿﻌﻬﺎ ﻋﻠﻲ ﺍﻟﺭﻛ ﺎﻡ‪ .‬ﺣ ﺭﻕ‬
‫ﺣﻠﻘﺎﺕ ﺍﻟﺗﺭﺷﻳﺢ ﺑﺈﺷﻌﺎﻟﻬﺎ ﺑﺎﻟﻛﺑﺭﻳﺕ ﺍﻭ ﻣﻭﻗﺩ ﺑﻧﺳﻥ‪ .‬ﺣﺳﺎﺏ ﻭﺯﻥ ﺍﻟﺭﻛﺎﻡ ﺍﻟﻣﺳﺗﺧﻠﺹ ﻓﻲ ﺍﻟﻭﻋﺎء )ﻭ‪  .(٢‬‬
‫‪ ‬ﺍﻟﻧﺗﺎﺋﺞ‪  :‬‬
‫ﺣﺳﺎﺏ ﻧﺳﺑﻪ ﺍﻟﺑﻳﺗﻭﻣﻳﻥ ﻓﻲ ﺍﻻﺧﺗﺑﺎﺭ ﻛﺎﻻﺗﻲ‪:‬‬
‫𝑊‬ ‫𝑊‬ ‫𝑊‬ ‫𝑊‬
‫𝑡𝑛𝑒𝑡𝑛𝑜𝐶 𝑛𝑒𝑚𝑢𝑡𝑖𝐵 ‪%‬‬ ‫‪𝑥100‬‬
‫𝑊‬ ‫𝑊‬
‫ﺣﻳﺙ‪:‬‬
‫ﻭ‪ = ١‬ﻭﺯﻥ ﻋﻳﻧﻪ ﺍﻻﺧﺗﺑﺎﺭ‪  ،‬‬
‫ﻭ‪ = 2‬ﻭﺯﻥ ﺍﻟﻣﺎء ﻓﻰ ﻋﻳﻧﻪ ﺍﻻﺧﺗﺑﺎﺭ‪،‬‬
‫ﻭ‪ = 3‬ﻭﺯﻥ ﺍﻟﺭﻛﺎﻡ ﺍﻟﻣﺳﺗﺧﻠﺹ‪،‬‬
‫ﻭ‪ = 4‬ﻭﺯﻥ ﺍﻟﻣﻭﺍﺩ ﺍﻟﻣﻌﺩﻧﻳﻪ ﻓﻲ ﺍﻟﻣﺳﺗﺧﻠﺹ‪.‬‬
‫‪ ‬‬
‫ﺗﺟﺭﺑﻪ ﺭﻗﻡ ‪  -16-‬‬
‫ﺍﻻﺧﺗﺑﺎﺭ ﺍﻟﻘﻳﺎﺳﻲ ﻟﺣﺳﺎﺏ ﻣﻌﺎﻣﻝ ﺍﻟﻣﺭﻭﻧﺔ ﺍﻟﺭﺟﻭﻋﻰ ﻟﻠﺗﺭﺑﺔ ﻭﺍﻟﺭﻛﺎﻡ ‪ ‬‬
‫‪Standard Test Method for Determining the Resilient Modulus of Soils and ‬‬
‫‪  Aggregate Materials‬‬
‫‪  AASHTOT307‐99‬‬
‫‪ ‬ﺍﻟﻐﺭﺽ ‪:‬‬
‫ﻣﻌﺎﻣﻝ ﺍﻟﻣﺭﻭﻧﺔ ﺍﻟﺭﺟﻭﻋﻰ ﻟﻠﺗﺭﺑﺔ ﻫﻭ ﺃﺣﺩ ﺍﻻﺧﺗﺑﺎﺭﺍﺕ ﺍﻟﻣﻌﻣﻠﻳﺔ ﺍﻟﺗﻲ ﻳﺣﺩﺩﻫﺎ ‪ AASHTO T307‐99‬ﺣﻳﺙ ﻫﻭ ﺍﺧﺗﺑﺎﺭ‬
‫ﺩﻳﻧﺎﻣﻳﻛﻲ ﻳﺗﻡ ﻓﻰ ﺧﻠﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ ﻟﺣﺳﺎﺏ ﻗﻳﻣﺔ ﻣﻌﺎﻣﻝ ﺍﻟﻣﺭﻭﻧﺔ ﺍﻟﺭﺟﻭﻋﻰ‪ .‬ﻗﻳﻣﺔ ﻣﻌﺎﻣﻝ ﺍﻟﻣﺭﻭﻧﺔ ﺍﻟﺭﺟﻭﻋﻰ ﻫﻭ ﻣﺅﺷﺭ‬
‫ﻋﻠﻰ ﻣﺭﻭﻧﺔ ﺍﻟﺭﻛﺎﻡ‪ ،‬ﺃﻭ ﺧﺎﺻﻳﺔ ﺍﻟﺗﺭﺑﺔ ﺍﻟﺗﻰ ﺗﺩﻝ ﻋﻠﻰ ﺍﻟﺗﻌﺎﻓﻲ ﻣﻥ ﺍﻹﺟﻬﺎﺩﺍﺕ ﺍﻟﻣﺗﻛﺭﺭﺓ ﻣﺛﻝ ﺗﻠﻙ ﺍﻟﻧﺎﺟﻣﺔ ﻋﻥ ﺍﻧﺣﻧﺎءﺍﺕ‬
‫ﺍﻟﺭﺻﻑ ﻧﺗﻳﺟﺔ ﻣﺭﻭﺭ ﻋﺟﻼﺕ ﺍﻟﻌﺭﺑﺎﺕ ﻋﻠﻰ ﺍﻟﻁﺭﻳﻖ ﻋﻠﻰ ﻣﺩﻯ ﻓﺗﺭﺓ ﻁﻭﻳﻠﺔ ﻣﻥ ﺍﻟﺯﻣﻥ‪ .‬ﺑﺷﻛﻝ ﻋﺎﻡ ﺗﺭﺗﺑﻁ ﻣﻭﺍﺩ ﺗﺭﺑﺔ‬
‫ﺍﻟﻁﺭﻳﻖ ﺍﻟﺗﺣﺗﻳﺔ ﺍﻟﺗﻲ ﺗﻅﻬﺭ ﻗﻳﻣﺔ ﻣﻌﺎﻣﻝ ﻣﺭﻭﻧﺔ ﻋﺎﻟﻳﺔ ﻣﻊ ﻁﺑﻘﺎﺕ ﺍﻟﺭﺻﻑ ﺍﻟﺗﻲ ﺗﺣﺎﻓﻅ ﻋﻠﻰ ﺳﻼﻣﺗﻬﺎ ﺩﻭﻥ ﺍﻟﺣﺎﺟﺔ ﺇﻟﻰ ﺗﺩﺍﺑﻳﺭ‬
‫ﺻﻳﺎﻧﺔ ﻏﻳﺭ ﻋﺎﺩﻳﺔ‪.‬‬
‫‪ ‬ﺍﻻﻫﻣﻳﺔ ﻭﺍﻻﺳﺗﺧﺩﺍﻡ ‪  :‬‬
‫ﻳﺗﻡ ﺇﺗﻣﺎﻡ ﺍﺧﺗﺑﺎﺭ ﻣﻌﺎﻣﻝ ﺍﻟﻣﺭﻭﻧﺔ ﺍﻟﺭﺟﻭﻋﻰ ﻣﻥ ﺧﻼﻝ ﺗﻁﺑﻳﻖ ﺳﻠﺳﻠﺔ ﻣﻥ ﻋﺩﺓ ﺁﻻﻑ ﻣﻥ ﺍﻷﺣﻣﺎﻝ ﺍﻟﺗﺭﺩﺩﻳﺔ ﺇﻟﻰ ﻋﻳﻧﺔ ﺭﻛﺎﻡ‬
‫ﻗﻁﺭﻫﺎ ‪ ١٥٠‬ﻣﻡ‪ .‬ﺍﻻﺧﺗﺑﺎﺭﺍﺕ ﺍﻟﺗﻰ ﺗﺗﻡ ﺑﻣﻭﺟﺏ ﻫﺫﺍ ﺍﻹﺟﺭﺍء ﺳﺗﻛﻭﻥ " ﺍﺧﺗﺑﺎﺭﺍﺕ ﺍﻟﻧﻭﻉ ﺍﻷﻭﻝ" ﺍﻟﺗﻲ ﺗﺧﺗﺹ ﺑﺎﻟﺗﺭﺑﺔ‪ ‬ﺍﻟﺣﺑﻳﺑﻳﺔ‪.‬‬
‫ﻋﻳﻧﺔ‪ ‬ﺍﻟﺗﺭﺑﺔ‪ ‬ﺍﻟﺗﻲ‪ ‬ﻳﺣﺩﺙ‪ ‬ﻟﺩﻳﻬﺎ‪ ‬ﺗﺷﻭﻩ‪ ‬ﻭﺧﺳﺎﺭﺓ‪ ‬ﻛﺑﻳﺭﺓ‪ ‬ﻓﻲ‪ ‬ﻁﻭﻝ‪ ‬ﺍﻟﻌﻳﻧﺔ‪ ‬ﻓﻲ‪ ‬ﻧﻬﺎﻳﺔ‪ ‬ﻫﺫﻩ‪ ‬ﺍﻻﺧﺗﺑﺎﺭﺍﺕ‪ ‬ﻳﻛﻭﻥ‪ ‬ﻟﻬﺎ‪ ‬ﻗﻳﻣﺔ‪ ‬ﻣﻌﺎﻣﻝ‪ ‬ﻣﺭﻭﻧﺔ‪ ‬‬
‫ﺑﻧﺳﺑﺔ‪ ‬ﻣﻧﺧﻔﺿﺔ‪ .‬ﺃﻣﺎ‪ ‬ﻋﻳﻧﺎﺕ‪ ‬ﺍﻟﺭﻛﺎﻡ ﺍﻟﺗﻲ ﺗﺗﻌﺎﻓﻰ ﻣﻥ ﻫﺫﻩ ﺍﻟﺗﺷﻛﻼﺕ ﻭﺗﻌﻭﺩ ﺇﻟﻰ ﻣﺎ ﻳﻘﺭﺏ ﻣﻥ ﻁﻭﻝ ﺍﻟﻌﻳﻧﺔ ﺍﻷﺻﻠﻲ ﺍﻟﻣﻘﺎﺱ ﻓﻲ‬
‫ﺑﺩﺍﻳﺔ ﺍﻻﺧﺗﺑﺎﺭ ﻳﻛﻭﻥ ﻟﻬﺎ ﻗﻳﻣﺔ ﻣﻌﺎﻣﻝ ﻣﺭﻭﻧﺔ ﻋﺎﻟﻳﺔ‪ .‬ﻭﻳﻣﻛﻥ ﺍﻟﺗﻌﺑﻳﺭ ﻋﻥ ﻗﻳﻣﺔ ﻣﻌﺎﻣﻝ ﺍﻟﻣﺭﻭﻧﺔ ﺍﻟﺭﺟﻭﻋﻰ ﺑﻭﺣﺩﺓ ‪  .MPa‬‬
‫ﻣﻬﻧﺩﺳﻳﻥ‪ ‬ﺍﻟﺗﺭﺑﺔ‪ ‬ﻗﺎﺩﺭﻭﻥ‪ ‬ﻋﻠﻰ‪ ‬ﺍﺳﺗﺧﺩﺍﻡ‪ ‬ﻣﻌﺎﻣﻝ‪ ‬ﺍﻟﻣﺭﻭﻧﺔ‪ ‬ﺍﻟﺭﺟﻭﻋﻰ‪ ‬ﻛﺄﺩﺍﺓ‪ ‬ﻟﺗﺻﻣﻳﻡ‪ ‬ﺍﻟﻁﺭﻕ‪ .‬ﻭﻳﻣﻛﻥ‪ ‬ﺃﻳﺿﺎ‪ ‬ﺃﻥ‪ ‬ﺗﺳﺗﺧﺩﻡ‪ ‬ﻛﺄﺩﺍﺓ‪ ‬ﻟﻠﺑﺣﺙ‪ ‬‬
‫ﻋﻥ‪ ‬ﺇﺟﺎﺑﺎﺕ‪ ‬ﻓﻲ‪ ‬ﺣﺎﻟﺔ‪ ‬ﺍﻟﻁﺭﻕ‪ ‬ﺍﻟﻣﻘﺎﻣﺔ‪ ‬ﺍﻟﺗﻲ‪ ‬ﺗﻅﻬﺭ‪ ‬ﻣﺷﺎﻛﻝ‪ ‬ﻓﻰ‪ ‬ﺍﻟﺭﺻﻑ‪ .‬ﺇﺟﺭﺍءﺍﺕ‪ ‬ﻣﻌﻣﻝ‪ ‬ﻫﻧﺩﺳﺔ‪ ‬ﺍﻟﻁﺭﻕ‪ ‬ﻭﺍﻟﻣﻁﺎﺭﺍﺕ‪ ‬ﺑﺟﺎﻣﻌﺔ‪ ‬‬
‫ﺍﻟﻣﻧﺻﻭﺭﺓ‪ ‬ﺗﺳﻣﺣﻠﻙ‪ ‬ﺑﺗﺷﻐﻳﻝ‪ ‬ﺍﺧﺗﺑﺎﺭ‪ ‬ﻣﻌﺎﻣﻝ‪ ‬ﺍﻟﻣﺭﻭﻧﺔ‪ ‬ﺍﻟﺭﺟﻭﻋﻰ‪ ‬ﻟﺗﺣﺩﻳﺩ‪ ‬ﻗﻳﻣﺗﻪ‪  .‬‬
‫‪ ‬ﺍﻻﺟﻬﺯﻩ ‪  :‬‬
‫‪ .A‬ﺟﻬﺎﺯ ‪  :UTM‬‬
‫‪ .١‬ﺇﻁﺎﺭ ﺍﻟﺗﺣﻣﻳﻝ ﺍﻟﺧﺎﺹ ﺑﺟﻬﺎﺯ ‪  .UTM‬‬
‫‪ .٢‬ﺧﻠﻳﺔ ﺍﻟﺗﺣﻣﻳﻝ ‪  .(5500 lbs.) 25 kN‬‬
‫‪ .B‬ﺧﻠﻳﺔ ﺍﻷﺑﺣﺎﺙ ﺍﻟﻬﻧﺩﺳﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ‪:‬‬
‫‪ .١‬ﺧﻠﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭﻭﺳﻳﺎﺝ ﺯﺟﺎﺟﻰ ﺷﺑﻛﻰ‪  .‬‬
‫‪ .٢‬ﻋﺩﺩ ‪ ٢‬ﻣﻘﻳﺎﺱ ﻟﻺﺳﺗﻁﺎﻟﺔ ﻟﻘﻳﺎﺱ ﺍﻟﺗﺷﻛﻼﻟﺧﻁﻰ ﻓﻰ ﺍﺭﺗﻔﺎﻉ ﺍﻟﻌﻳﻧﺔ‪  .‬‬
‫‪ .٣‬ﻟﻭﺣﺔ ﺍﻟﻘﺎﻋﺩﺓ ﻭﺍﻟﻣﺳﺎﻣﻳﺭ ﺍﻟﻣﻌﺩﻧﻳﺔ ﻟﺗﺛﺑﻳﺕ ﺍﻟﺧﻠﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ ﻓﻰ ﺇﻁﺎﺭ ﺍﻟﺗﺣﻣﻳﻝ ﻟﻠﺟﻬﺎﺯ‪  .‬‬
‫‪ .٤‬ﻋﺩﺩ ‪ ٢‬ﻛﺎﺑﻼﺕ ﺇﺷﺎﺭﺓ ﻟﻣﻘﺎﻳﻳﺱ ﺍﻻﺳﺗﻁﺎﻟﺔ‪  .‬‬
‫‪ .٥‬ﻣﺣﻭﻝ ﺿﺎﻏﻁ ﺍﻟﻬﻭﺍء ﻭﺧﻁ ﺇﻣﺩﺍﺩ ﺿﻐﻁ ﺍﻟﻬﻭﺍء‪.‬‬
‫‪ .C‬ﻣﻌﺩﺍﺕ ﺗﺟﻬﻳﺯ ﺍﻟﻌﻳﻧﺔ‪:‬‬
‫‪ .١‬ﻋﻳﻧﺎﺕ ﺍﻟﺗﺭﺑﺔ‪  .‬‬
‫‪ .٢‬ﻗﺎﻟﺏ ﺇﻋﺩﺍﺩ ﺍﻟﻌﻳﻧﺔ ﺍﻟﻣﻌﻧﻰ‪  .‬‬
‫‪ .٣‬ﻣﻁﺭﻗﺔ ﺑﺭﻭﻛﺗﻭﺭ ﺍﻟﻣﻌﺩﻝ ﻟﺩﻣﺞ ﺍﻟﻌﻳﻧﺔ)‪  .(10 lbs.‬‬
‫‪ .٤‬ﻣﻼﻋﻖ ﻭﻣﺳﺗﻘﻳﻡ ﺍﻟﺣﺎﻓﺔ ﻭﻣﺳﺗﻭﻯ‪  .‬‬
‫‪ .٥‬ﻭﺭﻧﻳﺔ ﻟﻘﻳﺎﺱ ﺍﻷﻁﻭﺍﻝ‪.‬‬
‫‪ .D‬ﻣﻌﺩﺍﺕ ﺗﺭﻛﻳﺏ ﻭﺗﺛﺑﻳﺕ ﺍﻟﻌﻳﻧﺔ‪:‬‬
‫‪ .١‬ﻗﺎﻟﺏ ﺗﻔﺭﻳﻎ ﺍﻟﻬﻭﺍء ﺫﻭ ﺍﻟﺷﻘﻳﻥ‪  .‬‬
‫‪ .٢‬ﻏﺷﺎء ﻣﻁﺎﻁﻰ ﻟﻌﻳﻧﺔ ‪ ١٥٠‬ﻣﻡ‪  .‬‬
‫‪ .٣‬ﺣﻠﻘﺎﺕ ﺩﺍﺋﺭﻳﺔ ﻟﺗﺛﺑﻳﺕ ﺍﻟﻐﺷﺎء ﺍﻟﻣﻁﺎﻁﻰ‪  .‬‬
‫‪ .٤‬ﻣﺿﺧﺔ ﺗﻔﺭﻳﻎ ﺍﻟﻬﻭﺍء‪  .‬‬
‫‪ .٥‬ﺃﻟﻭﺍﺡ ﻣﺳﺎﻣﻳﺔ ﺗﻭﺿﻊ ﺃﻋﻠﻰ ﻭﺃﺳﻔﻝ ﺍﻟﻌﻳﻧﺔ‪  .‬‬
‫‪ .٦‬ﻋﻳﻧﺔ ﺍﻟﻣﻌﺎﻳﺭﺓ ﺍﻟﻣﻁﺎﻁﻳﺔ ‪ ٢٠٠*١٠٠‬ﻣﻡ‪.‬‬
‫‪ .E‬ﺍﻟﻣﻌﺩﺍﺕ ﺍﻹﻟﻛﺗﺭﻭﻧﻳﺔ‪:‬‬
‫‪ .١‬ﺍﻟﺣﺎﺳﻭﺏ ﺍﻵﻟﻰ ‪ ‬‬
‫‪ .٢‬ﻭﺣﺩﺓ ﺗﺟﻣﻳﻊ ﺍﻟﺑﻳﺎﻧﺎﺕ‪  .‬‬
‫‪ .٣‬ﻭﺣﺩﺍﺕ ﺍﻟﺗﺣﻛﻡ‪.‬‬
‫ﺍﻟﺷ ﻛﻝ )‪ (١-١٦‬ﺇﻟ ﻰ ﺍﻟﺷ ﻛﻝ )‪ (١٣-١٦‬ﻳﻭﺿ ﺢ ﻣﻛﻭﻧ ﺎﺕ ﺟﻬ ﺎﺯ ‪ UTM‬ﻭﺍﻟﻣﻌ ﺩﺍﺕ ﺍﻟﻣﺳ ﺗﺧﺩﻣﺔ ﻓ ﻰ ﺇﺟ ﺭﺍء ﺍﻻﺧﺗﺑ ﺎﺭ ﺍﻟ ﻼﺯﻡ‬
‫ﻟﺣﺳﺎﺏ ﻣﻌﺎﻣﻝ‪ ‬ﺍﻟﻣﺭﻭﻧﺔ‪ ‬ﺍﻟﺭﺟﻭﻋﻰ‪ ‬ﻟﻠﺭﻛﺎﻡ‪.‬‬
‫‪ ‬‬

‫‪ .٢-١٦‬ﺇﻁﺎﺭ ﺍﻟﺗﺣﻣﻳﻝ ﺍﻟﺧﺎﺹ ﺑﺟﻬﺎﺯ ‪UTM‬‬ ‫‪ .١-١٦‬ﺟﻬﺎﺯ ‪UTM‬‬

‫‪ .٤-١٦‬ﺗﺟﻣﻳﻊ ﺍﺗﺻﺎﻝ ﻗﺿﻳﺏ ﺍﻟﺗﺣﻣﻳﻝ ﻭﻣﺣﻭﻝ ﺧﻁ ﺿﺎﻏﻁ‬


‫‪ .٣-١٦‬ﺧﻠﻳﺔ ﺍﻷﺑﺣﺎﺙ ﺍﻟﻬﻧﺩﺳﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ‬
‫ﺍﻟﻬﻭﺍء ﺑﺎﻟﺧﻠﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ‬
‫‪ .٧-١٦‬ﻭﺣﺩﺓ ﺗﺟﻣﻳﻊ ﺍﻟﺑﻳﺎﻧﺎﺕ ﻭﻭﺣﺩﺍﺕ‬ ‫‪ .٦-١٦‬ﻣﻘﻳﺎﺱ ﺍﻻﺳﺗﻁﺎﻟﺔ ﺍﻟﺧﻁﻰ ﻭﺧﻁ‬ ‫‪ .٥٫٣-١٦‬ﻟﻭﺣﺔﻗﺎﻋﺩﺓ ﺣﺩﻳﺩﻳﺔ ﻣﺗﻐﻳﺭﺓ‬
‫ﺍﻟﺗﺣﻛﻡ‬ ‫ﺇﻣﺩﺍﺩ ﺿﻐﻁ ﺍﻟﻬﻭﺍء‬ ‫ﺍﻻﺭﺗﻔﺎﻉ ﻟﺗﺛﺑﻳﺕ ﺍﻟﺧﻠﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ‬

‫‪ .٨-١٦‬ﺗﻭﺻﻳﻼﺕ ﺧﻁﻭﻁ ﺇﻣﺩﺍﺩ ﻭﺗﻔﺭﻳﻎ ﺿﻐﻁ ﺍﻟﻬﻭﺍء ﻟﻠﺧﻠﻳﺔ‬


‫‪ .٩-١٦‬ﺍﺗﺻﺎﻝ ﻣﻛﺑﺱ ﺍﻟﺟﻬﺎﺯ ﺑﺧﻠﻳﺔ ﺍﻟﺗﺣﻣﻳﻝ‬
‫ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ‬

‫‪ .١١-١٦‬ﻗﺎﻟﺏ ﻣﻌﺩﻧﻰ ﻭﺃﺩﻭﺍﺕ ﺇﻋﺩﺍﺩ ﺍﻟﻌﻳﻧﺔ‬ ‫‪ .١٠-١٦‬ﺟﻬﺎﺯ ﺗﺭﻛﻳﺏ ﺍﻟﻐﺷﺎء ﺍﻟﻣﻁﺎﻁﻰ ﻋﻠﻰ ﺍﻟﻌﻳﻧﺔ‬

‫‪ .١٣-١٦‬ﻋﻳﻧﺔ ﺍﻟﻣﻌﺎﻳﺭﺓ ﺍﻟﻣﻁﺎﻁﻳﺔ‬ ‫‪ .١٢-١٦‬ﺃﻟﻭﺍﺡ ﻣﺳﺎﻣﻳﺔ ﺗﻭﺿﻊ ﺃﻋﻠﻰ ﻭﺃﺳﻔﻝ ﺍﻟﻌﻳﻧﺔ‬


‫‪ ‬ﺗﺩﺭﻳﺏ‪ ‬ﻣﺳﺑﻖ‪ ‬ﻭﺍﻟﺧﺑﺭﺓ ‪:‬‬
‫ﺍﺧﺗﺑﺎﺭﻣﻌﺎﻣﻝ‪ ‬ﺍﻟﻣﺭﻭﻧﺔ‪ ‬ﺍﻟﺭﺟﻭﻋﻰ‪ ‬ﻫﻭﺇﺟﺭﺍء‪ ‬ﻣﻌﻣﻠﻰ‪ ‬ﻣﻌﻘﺩ‪ ‬ﻭﻣﺗﻁﻭﺭ‪ .‬ﻭﻣﻊ‪ ‬ﺫﻟﻙ‪ ،‬ﻫﻭﺍﺧﺗﺑﺎﺭﺫﻭ ﻧﺗﺎﺋﺞ ﻣﺭﺿﻳﺔ‪ ‬ﻋﻧﺩ ﺇﻧﺟﺎﺯﻩ ﺗﺑﻌﺎ‪ ‬‬
‫ﻟﻺﺟﺭﺍءﺍﺕ‪ ‬ﺍﻟﻘﻳﺎﺳﻳﺔ ﻟﻼﺧﺗﺑﺎﺭ‪ .AASHTO T307‐99 ‬ﻗﺑﻝ ﺇﺟﺭﺍء ﺍﻻﺧﺗﺑﺎﺭ ﻳﺟﺏ ﻋﻠﻰ ﻣﺟﺭﻯ ﺍﻻﺧﺗﺑﺎﺭ ﺃﻥ ﻳﻛﻭﻥ ﻋﻠﻰ ﺧﺑﺭﺓ‬
‫ﻭﺩﺭﺍﻳﺔ ﺑﺎﻵﺗﻰ‪:‬‬
‫‪ .١‬ﻁﺭﻕ ﺗﺻﻧﻳﻑ ﺍﻟﺗﺭﺑﺔ ﻭﺇﻋﺩﺍﺩ ﺍﻟﻌﻳﻧﺔ‪  .‬‬
‫‪ .٢‬ﺍﺧﺗﺑﺎﺭﺍﺕ ﺍﻟﺿﻐﻁ ﺍﻟﻣﺩﻋﻭﻣﺔ ﺟﺎﻧﺑﻳﺎ‪  .‬‬
‫‪ .٣‬ﻭﺿﻊ ﺍﻟﻌﻳﻧﺔ ﻓﻰ ﺍﻟﺧﻠﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ‪  .‬‬
‫‪ .٤‬ﺍﻟﻘﺩﺭﺓ ﻋﻠﻰ ﺗﺷﻐﻳﻠﻭﺗﻬﻳﺋﺔ ﺟﻬﺎﺯ ﺍﻻﺧﺗﺑﺎﺭ ‪  .UTM‬‬
‫‪ .٥‬ﺍﻟﺧﺑﺭﺓ ﺑﺄﺟﻬﺯﺓ ﺍﻟﺣﺎﺳﻭﺏ ﻭﺑﺭﻧﺎﻣﺞ ﺍﻟﺗﺷﻐﻳﻝ‪  .‬‬
‫ﻛﻝ ﻣﺎ ﺳﺑﻖ ﻳﺟﺏ ﺃﻥ ﻳﻛﺗﺳﺏ ﻣﻥ ﺧﻼﻝ ﺧﺑﺭﺍﺕ ﻋﺎﺩﻳﺔ ﻓﻰ ﻣﻌﻣﻝ ﺍﻟﺗﺭﺑﺔ ﺃﻣﺎ ﺟﻬﺎﺯ ‪ UTM‬ﻳﺣﺗﺎﺝ ﺇﻟﻰ ﺗﺩﺭﻳﺏ ﻣﻥ ﻧﻭﻉ‪ ‬ﺧﺎﺹ‪.‬‬
‫‪ ‬ﺧﻁﻭﺍﺕ ﺇﻋﺩﺍﺩ ﺍﻟﻌﻳﻧﺔ ‪:‬‬
‫ﻳﺟﺏ ﺍﻟﺗﺩﺭﻳﺏ ﻋﻠﻰ ﺇﻋﺩﺍﺩ ﺍﻟﻌﻳﻧﺔ ﺍﻟﻣﻁﺎﻁﻳﺔ ﻭﺇﺟﺭﺍء ﺍﻻﺧﺗﺑﺎﺭ ﻗﺑﻝ ﺇﻋﺩﺍﺩ ﻋﻳﻧﺔ ﺍﺧﺗﺑﺎﺭ ﺣﻘﻳﻘﻳﺔ ﻛﺎﻟﺗﺎﻟﻰ‪:‬‬
‫‪ .١‬ﺗﺳﺟﻳﻝ ﻛﻭﺩ ﺍﻟﻌﻳﻧﺔ ﻟﻼﺧﺗﺑﺎﺭ‪  .‬‬
‫‪ .٢‬ﺗﻌﻳﻳﻥ ﺍﻟﻭﺯﻥ ﺍﻟﻛﻠﻰ ﺍﻟﻣﻁﻠﻭﺏ ﻟﻌﻳﻧﺔ ﺍﻟﺭﻛﺎﻡ ﺑﻣﻌﻠﻭﻣﻳﺔ ﺍﻟﻛﺛﺎﻓﺔ ﺍﻟﺟﺎﻓﺔ ﺍﻟﻘﺻﻭﻯ ﻟﻠﺭﻛﺎﻡ ﻭﺣﺟﻡ ﺍﻟﻘﺎﻟﺏ ﺍﻟﻣﻌﺩﻧﻰ‪  .‬‬
‫‪ .٣‬ﺧﻠﻁ ﻋﻳﻧﺔ ﺍﻟﺭﻛﺎﻡ ﺍﻟﻐﻳﺭ ﻣﺩﻣﻭﻛﺔ ﺑﻧﺳﺑﺔ ﺍﻟﻣﻳﺎﻩ ﺍﻟﻣﺛﺎﻟﻳﺔ ﺍﻟﻣﻌﻳﻧﺔ ﺑﻭﺍﺳﻁﺔ ﺍﺧﺗﺑﺎﺭ ﺑﺭﻭﻛﺗﻭﺭ ﺍﻟﻣﻌﺩﻝ‪  .‬‬
‫‪ .٤‬ﻳﻭﺿﻊ ﺍﻟﺭﻛﺎﻡ ﻓﻰ ﺍﻟﻘﺎﻟﺏ ﻋﻠﻰ ﻫﻳﺋﺔ ‪ ٦‬ﻁﺑﻘﺎﺕ ﻭﺩﻣﻛﻬﺎ‪ ،‬ﻭﻳﺗﻡ ﺗﻌﻳﻳﻥ ﻭﺯﻥ ﺍﻟﺭﻛﺎﻡ ﺍﻟﻼﺯﻡ ﻟﻠﻁﺑﻘﺔ ﺍﻟﻭﺍﺣﺩﺓ ﻋﻥ ﻁﺭﻳﻖ ﻗﻳﻣﺔ‬
‫ﺍﻟﻭﺯﻥ ﺍﻟﻛﻠﻰ ﻟﻠﻌﻳﻧﺔ ﻋﻠﻰ ‪  .٦‬‬
‫‪ .٥‬ﺗﻌﻳﻳﻥ ﻋﺩﺩ ﺍﻟﺩﻗﺎﺕ ﺍﻟﻼﺯﻣﺔ ﻟﺩﻣﻙ ﻛﻝ ﻁﺑﻘﺔ ﻋﻥ ﻁﺭﻳﻖ ﺟﻬﺩ ﺍﻟﺩﻣﻙ ﺍﻟﻼﺯﻡ )‪ ١١٤‬ﺩﻗﺔ(‪  .‬‬
‫‪ .٦‬ﺗﺳﻭﻳﺔ ﺳﻁﺢ ﺍﻟﻌﻳﻧﺔ ﺍﻟﻧﻬﺎﺋﻰ ﻭﺇﺧﺭﺍﺟﻬﺎ ﻣﻥ ﺍﻟﻘﺎﻟﺏ ﺍﻟﻣﻌﺩﻧﻰ ﻭﺗﺳﺟﻳﻝ ﻁﻭﻝ ﻭﻗﻁﺭ ﻭﻭﺯﻥ ﺍﻟﻌﻳﻧﺔ‪  .‬‬
‫‪ .٧‬ﺍﻟﻌﻣﻝ ﺑﺣﺫﺭ ﻭﺳﺭﻋﺔ ﻟﺗﻔﺎﺩﻯ ﺍﻟﻔﻘﺩ ﻓﻰ ﻧﺳﺑﺔ ﺍﻟﺭﻁﻭﺑﺔ ﻓﻰ ﻋﻳﻧﺔ ﺍﻟﺭﻛﺎﻡ‪  .‬‬
‫‪ ‬ﺧﻁﻭﺍﺕ ﺗﺛﺑﻳﺕ ﺍﻟﻌﻳﻧﺔ‪ ‬ﻓﻰ ﺍﻟﺧﻠﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ ‪:‬‬
‫‪ .١‬ﻳﺗﻡ ﺍﻟﺗﻌﺎﻣﻝ ﻣﻊ ﻋﻳﻧﺔ ﺍﻟﺭﻛﺎﻡ ﺍﻟﻣﺩﻣﻭﻛﺔ ﻭﺍﻟﺧﻠﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ ﻋﻠﻰ ﻣﻧﺿﺩﺓ ﺗﺟﻬﻳﺯ ﺍﻟﻌﻳﻧﺎﺕ‪  .‬‬
‫‪ .٢‬ﻳﺗﻡ ﺇﺯﺍﻟﺔ ﺍﻟﺳﻳﺎﺝ ﺍﻟﺯﺟﺎﺟﻰ ﺍﻟﺷﺑﻛﻰ ﻟﻠﺧﻠﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ ﻭﺭﻓﻊ ﻭﺗﺛﺑﻳﺕ ﻣﻛﺑﺱ ﺍﻟﺧﻠﻳﺔ ﻟﻣﺳﺎﻓﺔ ﺍﻟﺧﻠﻭﺹ ﺍﻟﻘﺻﻭﻯ‪  .‬‬
‫‪ .٣‬ﺗﻭﺿﻊ ﻭﺭﻕ ﺗﺭﺷﻳﺢ ﺃﻋﻠﻰ ﻭﺃﺳﻔﻝ ﺳﻁﺢ ﺍﻟﻌﻳﻧﺔ‪ ،‬ﺛﻡ ﻳﻠﻳﻬﺎ ﺍﻷﻟﻭﺍﺡ ﺍﻟﻣﺳﺎﻣﻳﺔ ﻳﻌﻠﻭﻫﺎ ﺍﻷﻁﺑﺎﻕ ﺍﻹﺳﻁﻭﺍﻧﻳﺔ ﺍﻟﻣﻌﺩﻧﻳﺔ ﻟﻠﺧﻠﻳﺔ‬
‫ﻣﺛﺑﺕ ﻋﻠﻳﻬﺎ ﺣﻠﻘﺎﺕ ﺩﺍﺋﺭﻳﺔ ﻟﺗﺛﺑﻳﺕ ﺍﻟﻐﺷﺎء ﺍﻟﻣﻁﺎﻁﻰ‪  .‬‬
‫‪ .٤‬ﻳﺛﺑﺕ ﺍﻟﻐﺷﺎء ﺍﻟﻣﻁﺎﻁﻰ ﻋﻠﻰ ﻗﺎﻟﺏ ﺗﻔﺭﻳﻎ ﺍﻟﻬﻭﺍء ﺫﻭ ﺍﻟﺷﻘﻳﻥ‪ ،‬ﺛﻡ ﻳﻔﺭﻍ ﺍﻟﻬﻭﺍء ﻭﺗﺛﺑﺕ ﺍﻟﻌﻳﻧﺔ ﺑﺩﺍﺧﻝ ﺍﻟﻐﺷﺎء ﺍﻟﻣﻁﺎﻁﻰ‪  .‬‬
‫‪ .٥‬ﻳﻭﺿﻊ ﺍﻟﻘﺎﻟﺏ ﻭﺍﻟﻐﺷﺎء ﺍﻟﻣﻁﺎﻁﻰ ﻭﺍﻟﻌﻳﻧﺔ ﺑﺩﺍﺧﻝ ﺍﻟﺧﻠﻳﺔ ﺑﻳﻥ ﺍﻷﻁﺑﺎﻕ ﺍﻹﺳﻁﻭﺍﻧﻳﺔ ﺍﻟﻣﻌﺩﻧﻳﺔ ﺃﺛﻧﺎء ﻋﻣﻠﻳﺔ ﺗﻔﺭﻳﻎ ﺍﻟﻬﻭﺍء‪  .‬‬
‫‪ .٦‬ﻳﺣﺭﺭ ﻣﻛﺑﺱ ﺍﻟﺧﻠﻳﺔ ﻭﻳﺗﻡ ﺇﻧﺯﺍﻝ ﺍﻟﻁﺑﻖ ﺍﻹﺳﻁﻭﺍﻧﻰ ﺍﻟﻣﻌﺩﻧﻰ ﺍﻟﻌﻠﻭﻯ ﺣﺗﻰ ﻳﻼﻣﺱ ﺳﻁﺢ ﺍﻟﻌﻳﻧﺔ ﺛﻡ ﻳﺗﻡ ﺗﺛﺑﻳﺕ ﻣﻛﺑﺱ‬
‫ﺍﻟﺧﻠﻳﺔ ﻣﺭﺓ ﺃﺧﺭﻯ‪  .‬‬
‫‪ .٧‬ﺗﻠﻑ ﻧﻬﺎﻳﺎﺕ ﺍﻟﻐﺷﺎء ﺍﻟﻣﻁﺎﻁﻰ ﺣﺗﻰ ﺗﻐﻁﻰ ﺍﻷﻁﺑﺎﻕ ﺍﻹﺳﻁﻭﺍﻧﻳﺔ ﺍﻟﻣﻌﺩﻧﻳﺔ ﺍﻟﻌﻠﻭﻯ ﻭﺍﻟﺳﻔﻠﻰ‪ ،‬ﻭﻳﺗﻡ ﺇﺣﻛﺎﻣﻬﺎ ﺑﻭﺍﺳﻁﺔ‬
‫ﺍﻟﺣﻠﻘﺎﺕ ﺍﻟﺩﺍﺋﺭﻳﺔ‪  .‬‬
‫‪ .٨‬ﻳﺣﺭﺭ ﺗﻔﺭﻳﻎ ﺍﻟﺿﻐﻁ‪ ،‬ﻭﻳﻔﺻﻝ ﻭﻳﺯﺍﻝ ﻗﺎﻟﺏ ﺗﺛﺑﻳﺕ ﺍﻟﻐﺷﺎء ﺍﻟﻣﻁﺎﻁﻰ‪  .‬‬
‫‪ .٩‬ﻳﺗﻡ ﺇﻧﺯﺍﻝ ﺍﻟﺳﻳﺎﺝ ﺍﻟﺯﺟﺎﺟﻰ ﺍﻟﺷﺑﻛﻰ ﻟﻠﺧﻠﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ ﻭﻏﻠﻖ ﻭﺗﺛﺑﻳﺕ ﻣﺣﺎﺑﺱ ﺍﻷﻣﺎﻥ‪  .‬‬
‫‪ .١٠‬ﻓﺗﺢ ﻛﻝ ﺧﻁﻭﻁ ﺻﻣﺎﻣﺎﺕ ﺍﻟﺗﺻﺭﻳﻑ ﻣﻥ ﺍﻟﻌﻳﻧﺔ ﻟﻠﻬﻭﺍء ﺍﻟﺟﻭﻯ‪  .‬‬
‫‪ .١١‬ﺗﺛﺑﺕ ﻛﻼ ﻣﻘﺎﻳﻳﺱ ﺍﻻﺳﺗﻁﺎﻟﺔ ﺍﻟﺧﻁﻳﺔ ﻭﻣﺣﻭﻝ ﺿﺎﻏﻁ ﺍﻟﻬﻭﺍء ﻭﺧﻁ ﺇﻣﺩﺍﺩ ﺿﻐﻁ ﺍﻟﻬﻭﺍء‪  .‬‬
‫‪ ‬ﺗﺭﻛﻳﺏ ﺍﻟﺧﻠﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ ﺑﺩﺍﺧﻝ ﺇﻁﺎﺭﺍﻟﺗﺣﻣﻳﻝ ﺍﻟﺧﺎﺹ ﺑﺟﻬﺎﺯ‪: UTM ‬‬
‫‪ .١‬ﺗﺛﺑﺕ ﻟﻭﺣﺔ ﺍﻟﻘﺎﻋﺩﺓ ﺍﻟﻣﻌﺩﻧﻳﺔ ﻋﻧﺩ ﺍﺭﺗﻔﺎﻉ ﻣﻧﺎﺳﺏ ﻓﻰ ﺇﻁﺎﺭﺍﻟﺗﺣﻣﻳﻝ ﺍﻟﺧﺎﺹ ﺟﻬﺎﺯ ‪  .UTM‬‬
‫‪ .٢‬ﺗﺭﻓﻊ ﻭﺻﻠﺔ ﺫﺭﺍﻉ ﺍﻟﻣﻛﺑﺱ ﺑﺫﺭﺍﻉ ﺍﻟﺗﻭﺻﻳﻝ ﻟﻠﺳﻣﺎﺡ ﺑﺧﻠﻭﺹ ﻛﺎﻓﻰ ﻟﺗﺛﺑﻳﺕ ﺍﻟﺧﻠﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ‪  .‬‬
‫‪ .٣‬ﻳﺟﺏ ﺍﻟﺗﺄﻛﺩ ﻣﻥ ﺃﻥ ﺧﻠﻳﺔ ﺍﻟﺗﺣﻣﻳﻝ ﻣﺛﺑﺗﺔ ﻭﻣﻭﺻﻠﺔ ﺗﻭﺻﻳﻝ ﺻﺣﻳﺢ‪  .‬‬
‫‪ .٤‬ﻳﺗﻡ ﺗﺭﻛﻳﺏ ﻭﻭﺿﻊ ﺍﻟﺧﻠﻳﺔ ﻓﻰ ﺇﻁﺎﺭ ﺍﻟﺗﺣﻣﻳﻝ ﺍﻟﺧﺎﺹ ﺑﺟﻬﺎﺯ ‪ UTM‬ﻋﻠﻰ ﻟﻭﺣﺔ ﺍﻟﻘﺎﻋﺩﺓ ﺍﻟﻣﻌﺩﻧﻳﺔ‪  .‬‬
‫‪ .٥‬ﺑﺎﺳﺗﺧﺩﺍﻡ ﻣﻛﺑﺱ ﺍﻟﺟﻬﺎﺯ ﻳﺗﻡ ﺇﻧﺯﺍﻝ ﻭﺻﻠﺔ ﺫﺭﺍﻉ ﺍﻟﻣﻛﺑﺱ ﺑﺫﺭﺍﻉ ﺍﻟﺗﻭﺻﻳﻝ ﺣﺗﻰ ﻳﺗﻘﻠﺹ ﺍﻟﺧﻠﻭﺹ ﺇﻟﻰ ﺣﻭﺍﻟﻰ ‪ ١‬ﺳﻡ‪  .‬‬
‫‪ .٦‬ﺑﺎﺳﺗﺧﺩﺍﻡ )‪ (ATS controller in STROKE control‬ﻳﺗﻡ ﺍﻟﺗﺣﻛﻡ ﻓﻰ ﺇﻧﺯﺍﻝ ﻭﺻﻠﺔ ﺫﺭﺍﻉ ﺍﻟﻣﻛﺑﺱ ﺑﺫﺭﺍﻉ ﺍﻟﺗﻭﺻﻳﻝ‬
‫ﺣﺗﻰ ﻳﺗﻁﺎﺑﻖ ﻧﻬﺎﻳﺔ ﻗﺿﻳﺏ ﺍﻟﺗﺣﻣﻳﻝ ﻋﻠﻰ ﺳﻁﺢ ﺍﻟﻁﺑﻖ ﺍﻹﺳﻁﻭﺍﻧﻲ ﺍﻟﻣﻌﺩﻧﻲ ﺍﻟﻌﻠﻭﻯ‪  .‬‬
‫‪ .٧‬ﺗﺭﺑﻁ ﻣﺣﺎﺑﺱ ﺍﻷﻣﺎﻥ ﻟﺿﻣﺎﻥ ﺗﺄﻣﻳﻥ ﺍﻟﺧﻠﻳﺔ‪ ،‬ﻭﻳﺗﻡ ﺗﻭﺻﻳﻝ ﺧﻁ ﺇﻣﺩﺍﺩ ﺿﻐﻁ ﺍﻟﻬﻭﺍء ﻭﻣﺣﻭﻝ ﺿﺎﻏﻁ ﺍﻟﻬﻭﺍء ﻭﻛﺎﺑﻼﺕ‬
‫ﺗﻭﺻﻳﻝ ﻣﻘﺎﻳﻳﺱ ﺍﻻﺳﺗﻁﺎﻟﺔ ﺍﻟﺧﻁﻳﺔ‪.‬‬
‫‪ ‬ﺍﻋﺩﺍﺩ ﺍﻻﺧﺗﺑﺎﺭ‪  :‬‬
‫‪ .١‬ﻓﻲ ﺧﻼﻝ ﺍﻟﻭﻗﺕ ﺍﻟﻼﺯﻡ ﻟﺗﺟﻬﻳﺯ ﺍﻟﻌﻳﻧﺔ ﻭﺗﻭﺻﻳﻝ ﺍﻟﺧﻠﻳﺔ ﺑﺟﻬﺎﺯ ‪ UTM‬ﻳﺗﻡ ﺗﺷﻐﻳﻝ ﻣﺿﺧﺔ ﺍﻟﻬﻭﺍء ﺣﺗﻰ ﺗﻌﻣﻝ ﻋﻠﻰ ﺍﺣﻣﺎء‬
‫ﺍﻟﻧﻅﺎﻡ ﺍﻟﻬﻳﺩﺭﻭﻟﻳﻛﻲ ‪  .‬‬
‫‪ .٢‬ﻳﺗﻡ ﺿﺑﻁ ﻗﺭﺍءﺍﺕ ﻣﻘﺎﻳﻳﺱ ﺍﻻﺳﺗﻁﺎﻟﺔ ﺍﻟﺧﻁﻳﺔ ﺍﻟﻰ ﺍﻟﺻﻔﺭ ﻳﺩﻭﻳﺎ ﺑﺎﺳﺗﺧﺩﺍﻡ ﺑﺭﻧﺎﻣﺞ )‪  . (ATS controller‬‬
‫‪ .٣‬ﻳﺗﻡ ﺍﻟﺗﺄﻛﺩ ﻣﻥ ﺣﺩﻭﺩ ﺍﻷﺣﻣﺎﻝ ﻭﺍﻟﻧﻅﺎﻡ ﺍﻟﻬﻳﺩﺭﻭﻟﻳﻛﻲ ﺑﺣﻳﺙ ﻳﺗﻡ ﻏﻠﻖ ﺍﻟﻧﻅﺎﻡ ﺃﺗﻭﻣﺎﺗﻳﻛﻳﺎ ﻋﻧﺩ ﺗﺧﻁﻲ ﻗﺭﺍءﺍﺕ ﺍﻷﺣﻣﺎﻝ‬
‫ﻭﺍﻟﺗﺷﻛﻝ ﻗﺩﺭﺓ ﺳﻌﺔ ﺍﻟﺧﻠﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ‪  .‬‬
‫‪ .٤‬ﻳﺗﻡ ﺍﺧﺗﻳﺎﺭ ﻧﻭﻉ ﺍﻻﺧﺗﺑﺎﺭ ﺍﻟﻣﻧﺎﺳﺏ ﻟﺣﺳﺎﺏ ﻣﻌﺎﻣﻝ ﺍﻟﻣﺭﻭﻧﺔ ﺍﻟﺭﺟﻭﻋﻲ ﻭﺍﺩﺧﺎﻝ ﻛﺎﻓﺔ ﺍﻟﺑﻳﺎﻧﺎﺕ ﺍﻟﻼﺯﻣﺔ ﻻﺟﺭﺍء ﺍﻻﺧﺗﺑﺎﺭ‬
‫ﻭﺍﻟﻌﻳﻧﺔ ﻓﻲ ﺍﻟﺑﺭﻧﺎﻣﺞ ‪  .‬‬
‫‪ .٥‬ﺗﺣﺭﻳﺭ ﻣﻛﺑﺱ ﺍﻟﺧﻠﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ‪  .‬‬
‫‪ ‬ﺍﺟﺭﺍء ﺍﺧﺗﺑﺎﺭ ﻣﻌﺎﻣﻝ ﺍﻟﻣﺭﻭﻧﺔ ﺍﻟﺭﺟﻭﻋﻲ ‪  :‬‬
‫‪ .١‬ﺍﺧﺗﻳﺎﺭ "‪ "Start test‬ﻓﻲ ﻗﺎﺋﻣﺔ ﺍﻟﺑﺭﻧﺎﻣﺞ )‪  .(ATS controller‬‬
‫‪ .٢‬ﺳﻭﻑ ﻳﻘﻭﻡ ﺍﻟﺟﻬﺎﺯ ﺑﺎﻟﺑﺩء ﻓﻲ ﺗﻁﺑﻳﻖ ﻧﻅﺎﻡ ﺍﻟﺗﺣﻣﻳﻝ ﻋﻠﻲ ﺍﻟﻌﻳﻧﺔ ﻁﺑﻘﺎ ﻟﻣﻭﺍﺻﻔﺔ ﺍﻻﺧﺗﺑﺎﺭ‪ ،‬ﺣﻳﺙ ﺗﺑﺩﺃ ﻣﺭﺣﻠﺔ‬
‫)‪ (preconditioning stage‬ﺑﻌﺩﺩ )‪ (١٠٠٠ : ٥٠٠‬ﺩﻭﺭﺓ ﺗﺣﻣﻳﻝ )‪ ١‬ﺙ‪ /‬ﺍﻟﺩﻭﺭﺓ( ﺑﺿﻐﻁ ﺇﺣﺎﻁﺔ ﻣﻘﺩﺍﺭﺓ ‪١٠٣٫٤‬‬
‫‪ ، kPa‬ﻳﺟﺏ ﺃﻻ ﺗﻘﻝ ﻋﺩﺩ ﻧﻘﺎﻁ ﺍﻟﺑﻳﺎﻧﺎﺕ ﺍﻟﻣﺳﺟﻠﺔ ﺑﻣﻘﺎﻳﻳﺱ ﺍﻻﺳﺗﻁﺎﻟﺔ ﻋﻥ ‪ ٢٠٠‬ﻧﻘﻁﺔ ﻟﻛﻝ ﺩﻭﺭﺓ‪  .‬‬
‫‪ .٣‬ﺑﻌﺩ ﺍﻻﻧﺗﻬﺎء ﻣﻥ ﻣﺭﺣﻠﺔ )‪ (preconditioning stage‬ﺗﺑﺩﺃ ﻣﺭﺍﺣﻝ ﺍﻟﺗﺣﻣﻳﻝ )‪ ١٥‬ﻣﺭﺣﻠﺔ( ﻁﺑﻘﺎ ﻟﻠﻣﻭﺍﺻﻔﺔ ﺑﻭﺍﻗﻊ‬
‫‪ ١٠٠‬ﺩﻭﺭﺓ ﺗﺣﻣﻳﻝ ﻟﻛﻝ ﻣﺭﺣﻠﺔ‪  .‬‬
‫‪ .٤‬ﻳﺟﺏ ﻋﻠﻲ ﻣﺟﺭﻯ ﺍﻻﺧﺗﺑﺎﺭ ﻣﺭﺍﻋﺎﻩ ﺍﻻﺗﻲ ) ﺃﻻ ﻳﺯﻳﺩ ﺍﻻﻧﻔﻌﺎﻝ ﺍﻟﻣﺣﻭﺭﻱ ﺍﻟﺩﺍﺋﻡ ﻋﻥ ‪ %٥‬ﺧﻼﻝ ﻓﺗﺭﻩ ﺍﻻﺣﻣﺎء ﻣﺎ ﻗﺑﻝ‬
‫ﺍﻻﺧﺗﺑﺎﺭ ﻭ ﺇﻻ ﻳﺗﻡ ﺍﻳﻘﺎﻑ ﺍﻻﺧﺗﺑﺎﺭ‪ -‬ﻳﺟﺏ ﺍﻥ ﺗﻛﻭﻥ ﻗﺭﺍءﺍﺕ ﻣﻘﺎﻳﻳﺱ ﺍﻻﺳﺗﻁﺎﻟﺔ ﺍﻟﺧﻁﻳﺔ ﻣﺗﻘﺎﺭﺏ ﻁﺑﻘﺎ ﻟﻠﻣﻭﺍﺻﻔﺔ‪ -‬ﻣﺭﺍﻗﺑﺔ‬
‫ﻗﻳﻣﺔ ﺍﻟﺣﻣﻝ ﺍﻟﻔﻌﻠﻲ ﻋﻠﻰ ﺍﻟﻌﻳﻧﺔ ﺃﺛﻧﺎء ﺇﺟﺭﺍء ﺍﻻﺧﺗﺑﺎﺭ(‪  .‬‬
‫‪ .٥‬ﻋﻧﺩ ﺍﻻﻧﺗﻬﺎء ﻣﻥ ﺍﻻﺧﺗﺑﺎﺭ ﻳﺗﻡ ﺗﺟﻣﻳﻊ ﺑﻳﺎﻧﺎﺕ ﺍﻻﺧﺗﺑﺎﺭ ﻭ ﻣﻥ ﺛﻡ ﻳﺗﻡ ﺇﻋﺩﺍﺩ ﺍﻟﺗﻘﺭﻳﺭ ﺍﻟﻔﻧﻲ ﻣﺗﺿﻣﻧﺎ ﻗﻳﻡ ﻣﻌﺎﻣﻝ ﺍﻟﻣﺭﻭﻧﺔ‬
‫ﺍﻟﺭﺟﻭﻋﻲ ﻭ ﻛﺫﻟﻙ ﺣﺳﺎﺑﺎﺕ ﺍﻟﻼﻳﻘﻳﻥ ﻭ ﺍﺭﻓﺎﻗﻬﺎ ﺑﺎﻟﺗﻘﺭﻳﺭ ﺑﻧﺎء ﻋﻠﻰ ﻁﻠﺏ ﺍﻟﻌﻣﻳﻝ‪  .‬‬
‫‪ .٦‬ﺑﻌﺩ ﺍﻟﺣﺻﻭﻝ ﻋﻠﻲ ﺍﻟﻧﺗﺎﺋﺞ ﻣﻥ ﺍﻟﺟﻬﺎﺯ‪ ،‬ﻳﺗﻡ ﺍﻏﻼﻕ ﺍﻟﻧﻅﺎﻡ ﺍﻟﻬﻳﺭﻭﻟﻳﻛﻲ ﻟﻠﺟﻬﺎﺯ ﻭ ﻣﺿﺧﺔ ﺍﻟﻬﻭﺍء ﺛﻡ ﺍﻏﻼﻕ ﻭﺣﺩﺓ ﺗﺟﻣﻳﻊ‬
‫ﺍﻟﺑﻳﺎﻧﺎﺕ ﻭ ﺍﻟﺣﺎﺳﻭﺏ‪  .‬‬
‫‪ .٧‬ﻳﺗﻡ ﺇﺯﺍﻟﺔ ﺍﻟﺧﻠﻳﺔ ﺛﻼﺛﻳﺔ ﺍﻟﻣﺣﺎﻭﺭ ﻣﻥ ﺍﻟﺟﻬﺎﺯ ﻭ ﺇﺧﺭﺍﺝ ﺍﻟﻌﻳﻧﺔ ﺍﻟﻣﺧﺗﺑﺭﺓ ﻭﺍﻟﺗﺄﻛﺩ ﻣﻥ ﺍﻟﻣﺣﺗﻭﻯ ﺍﻟﻣﺎﺋﻰ ﻟﻠﻌﻳﻧﺔ‪  .‬‬
‫‪ .٨‬ﻓﻰ ﺣﺎﻟﺔ ﺣﺩﻭﺙ ﺃﻯ ﺗﺻﺭﻑ ﻏﻳﺭ ﻁﺑﻳﻌﻰ ﺃﺛﻧﺎء ﺇﺟﺭﺍء ﺍﻻﺧﺗﺑﺎﺭ ﻳﺗﻡ ﺍﺳﺗﺧﺩﺍﻡ ﺯﺭﺍﺭ ﺇﻳﻘﺎﻑ ﺍﻟﻁﻭﺍﺭﺉ ﻟﻭﻗﻑ ﺍﻻﺧﺗﺑﺎﺭ‬
‫ﻟﺣﻣﺎﻳﺔ ﺍﻟﻌﻳﻧﺔ ﻭﺍﻟﺟﻬﺎﺯ‪  .‬‬
‫‪ .٩‬ﻓﻰ ﺣﺎﻟﺔ ﺃﻥ ﻳﻘﻑ ﺍﻻﺧﺗﺑﺎﺭ ﺗﻠﻘﺎﺋﻳﺎ ﺑﻣﺟﺭﺩ ﺍﻟﺿﻐﻁ ﻋﻠﻰ ﺯﺭ ﺍﻟﺗﺷﻐﻳﻝ ﻟﺑﺩء ﺍﻻﺧﺗﺑﺎﺭ ﻓﺫﻟﻙ ﻳﻌﻭﺩ ﺇﻟﻰ ﺧﺭﻭﺝ ﺃﺣﺩ ﻗﺭﺍءﺍﺕ‬
‫ﺍﻟﺣﻣﻝ ﺃﻭ ﺍﻻﺳﺗﻁﺎﻟﺔ ﺧﺎﺭﺝ ﺍﻟﺣﺩﻭﺩ ﺍﻟﻣﺳﻣﻭﺣﺔ ﺍﻟﻣﻌﺭﻓﺔ ﺩﺍﺧﻝ ﺍﻟﺑﺭﻧﺎﻣﺞ‪ ،‬ﻓﻰ ﻫﺫﻩ ﺍﻟﺣﺎﻟﺔ ﻳﺗﻡ ﺇﻋﺎﺩﺓ ﺿﺑﻁ ﺍﻟﻘﺭﺍءﺍﺕ ﻋﻠﻰ‬
‫ﺍﻟﺻﻔﺭ ﻟﻠﺳﻣﺎﺡ ﻟﻠﺑﺭﻧﺎﻣﺞ ﺑﺎﻟﺑﺩء ﻓﻰ ﺍﻻﺧﺗﺑﺎﺭ‪  .‬‬
‫ﺍﻟﺷﻛﻝ )‪ (١٤-١٦‬ﻣﻠﺧﺹ ﻟﻠﺧﻁﻭﺍﺕ ﺍﻟﺳﺎﺑﻖ ﺫﻛﺭﻫﺎ ﻹﺟﺭﺍء ﺍﻻﺧﺗﺑﺎﺭ‪.‬‬
‫‪ ‬‬