0% found this document useful (0 votes)
45 views1 page

K 250 Purnabakti Karya Bintan

This document provides a concrete mix design for a normal mix concrete with a specified compressive strength of 250 kg/cm2 at 28 days. The mix uses local materials including cement, fine aggregate from Anambas sand, and coarse aggregate from Tanjung Balai Karimun crushed stone. The mix is designed with a water-cement ratio of 0.545, 330 kg/m3 of cement, 180 liters of water, 830 kg/m3 of fine aggregate, and 1015 kg/m3 of coarse aggregate to achieve a target mean strength of 299 kg/cm2 and designed density of 2355 kg/m3. The mix is specified to have a 100±25 mm slump and

Uploaded by

Arda S Ars
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
0% found this document useful (0 votes)
45 views1 page

K 250 Purnabakti Karya Bintan

This document provides a concrete mix design for a normal mix concrete with a specified compressive strength of 250 kg/cm2 at 28 days. The mix uses local materials including cement, fine aggregate from Anambas sand, and coarse aggregate from Tanjung Balai Karimun crushed stone. The mix is designed with a water-cement ratio of 0.545, 330 kg/m3 of cement, 180 liters of water, 830 kg/m3 of fine aggregate, and 1015 kg/m3 of coarse aggregate to achieve a target mean strength of 299 kg/cm2 and designed density of 2355 kg/m3. The mix is specified to have a 100±25 mm slump and

Uploaded by

Arda S Ars
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
You are on page 1/ 1

JOB MIX DESIGN

CONCRETE MIX DESIGN FOR : Normal Mix CONCRETE CLASS : K 250


PROJECT : :Machine
Lanjutan Pembangunan
Room Puskesmas
& Infrastructure DATE : 08 Oktober 2020
: Siantan Timur No : 20201008-2
MATERIAL : Semen Conch/ Tiga Roda
: Pasir Lokal Anambas
: Batu Split Tanjung Balai Karimun
CONTRACTOR : PT. PURNABAKTI KARYA BINTAN

ITEM REMAKS VALUES


1 Characteristic Strength ( Specified ) 250 Kg/Cm2 Compressive at 28 days
2 Standard Deviation 30 Kg/Cm2
3 Margin ( K = 1.64 ) 1.64 x 30 = 49 Kg/Cm2
4 Target Mean Strength 250 + 49 = 299 Kg/Cm2
5 Free - Water / Cemen Ratio 0.545 Use the Lower Value
6 Cement Type ( Brant ) ( Specified ) PCC ( Bag )
7 Aggragate Type : Fine Uncrushed
Aggragate Type : Coarse Crushed
8 Non Admixture
9 Specific Gravity of Cement 3.10 Known
10 Specific Gravity of Fine aggregate ( S. S. D ) 2.59 Known
11 Specific Gravity of Coarse aggregate ( S. S. D ) 2.65 Known
12 Maximum aggregat Size ( Specified ) 20 mm
13 Granding of Fine aggregate ( B.S 882 ) Zone Two
14 Proportion of Fine aggregate 45%
15 Specific gravity of combined Aggregate ( 2.59 x 45% ) + (2.65 x 55% ) = 2.623
16 Slump ( Specified ) 100 ± 25 mm
17 Air Content ( Estimated ) 1 % = 10 Litres Abs./M3
18 Free Water Reguirement 180 Lit./M3 = 180 Litres Abs./M3
19 Cemen Content 180 : 0.545 = 330 Kg/M3
20 Adopted Cement content 330 Kg/M3 = 106.45 litres Abs./ M3
21 Total Aggregate Content 1000 -10 - 180 - 106.45 = 703.55 Litres Abs./M3
1845 Kg/M3
22 Fine Aggregate Content 1845 x 45% = 830 Kg/M3
23 Coarse Aggregate Content 1845 - 830 = 1015 Kg/M3
24 Designed Density of Concrete 330 + 180 + 1845 = 2355 Kg/M3

SUMMARY OF BATCH WEIGHTS ( SSD ) PER CUBIC METRE OF CONCRETE


DESIGN VOL CEMENT WATER FINE COARSE
Cu. Liter PCC TAP Zone Two 20 mm

1 ( One ) 330 Kg 180 Liter 830 Kg 1015 Kg

WIDODO CANDRA
WAKIL DIREKTUR

Jl. Imam Hasanudin No.6, RT.001 RW.003 Kel. Ranai Kec. Bunguran Timur